Difference between revisions of "Stepper Recipes"
m (→DUV-42P-6: updated spin speed / noted mistake) |
|||
(34 intermediate revisions by 5 users not shown) | |||
Line 1: | Line 1: | ||
{{recipes|Lithography}} |
{{recipes|Lithography}} |
||
+ | [[category: Lithography]] |
||
+ | Below is a listing of stepper lithography recipes. |
||
− | Below is a listing of stepper lithography recipes. Stepper 1 and Stepper 2 are i-line systems with good piece handling capabilities. Stepper 3 is a DUV (248nm) system. DUV resists do not work for i-line and i-line resists do not work for DUV. Based on your sample reflectivity, absorption (or whether or not you use an ARC layer), and surface topography the exposure time / focus offset parameters may vary. This listing is a guideline to get you started. The recipes are tabulated to give you the values of the key parameters you will need to establish your recipe. Underlayers such as LOL2000 or PMGI can be used on the stepper systems. See the underlayer datasheets for details. Post develop bakes (not listed) are used to make the resist more etch resistant and depend on subsequent processes. Care should be taken with post development bakes as resist reflow can occur. Unless otherwise noted, all exposures are done on flat, silicon wafers. |
||
+ | Stepper 1 and Stepper 2 are i-line systems with good piece handling capabilities. Stepper 3 is a DUV (248nm) system primarily used for full 100mm wafers. DUV resists do not work for i-line and i-line resists do not work for DUV. Based on your sample reflectivity, absorption (or whether or not you use an ARC layer), and surface topography, the exposure time / focus offset parameters may vary. |
||
+ | This listing is a guideline to get you started. For critical lithography steps, you should run your own exposure and/or focus array to determine the proper parameters. |
||
− | Parameters are indicated in separate tables for each stepper system. Multiply the exposure times by 0.30 (from the 6300 system) to get a starting exposure time for the GCA Autostep200 system. You will need to do a focus and/or exposure array to get optimal process parameters. |
||
+ | The recipes are tabulated to give you the values of the key parameters you will need to establish your recipe. Underlayers such as LOL2000 or PMGI can be used on the stepper systems. See the underlayer datasheets for details. Post develop bakes (not listed) are used to make the resist more etch resistant and depend on subsequent processes. Care should be taken with post development bakes as resist reflow can occur. Unless otherwise noted, all exposures are done on flat, silicon wafers. |
||
− | = [[Stepper 1 (GCA 6300)]] = |
||
+ | |||
+ | Parameters are indicated in separate tables for each stepper system. |
||
+ | |||
+ | =[[Stepper 1 (GCA 6300)]]= |
||
+ | |||
+ | Multiply the GCA 6300 exposure times by 0.30 to get a starting exposure time for the GCA Autostep200 system. |
||
==Positive Resist (GCA 6300)== <!--Note that if this heading is changed, the recipe links on the Lithography page must be changed--> |
==Positive Resist (GCA 6300)== <!--Note that if this heading is changed, the recipe links on the Lithography page must be changed--> |
||
Line 11: | Line 19: | ||
Unless otherwise noted, bakes are on hot plates. For recipes with CEM, the CEM is spun on after the first resist bake, exposure is then done, and the CEM is rinsed off with DI water before the PEB. CEM generally improves resolution and process tolerance at the expense of higher exposure time. |
Unless otherwise noted, bakes are on hot plates. For recipes with CEM, the CEM is spun on after the first resist bake, exposure is then done, and the CEM is rinsed off with DI water before the PEB. CEM generally improves resolution and process tolerance at the expense of higher exposure time. |
||
− | {| |
+ | {| class="wikitable" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center;" border="1" |
|- bgcolor="#D0E7FF" |
|- bgcolor="#D0E7FF" |
||
− | ! width="100" | |
+ | ! width="100" |Resist |
− | ! width="100" | |
+ | ! width="100" |Spin Cond. |
− | ! width="75" | |
+ | ! width="75" |Bake |
− | ! width="75" | |
+ | ! width="75" |Thickness |
− | ! width="125" | |
+ | ! width="125" |Exposure Time |
− | ! width="100" | |
+ | ! width="100" |Focus Offset |
− | ! width="75" | |
+ | ! width="75" |PEB |
− | ! width="100" | |
+ | ! width="100" |Developer |
− | ! width="125" | |
+ | ! width="125" |Developer Time |
− | ! width="300" | |
+ | ! width="300" |Comments |
|- |
|- |
||
− | | |
+ | |SPR955CM0.9 |
− | | |
+ | |3 krpm/30” |
− | | |
+ | |95°C/60” |
− | | |
+ | |~ 0.9 um |
− | | |
+ | |1.2” |
− | | |
+ | |0 |
− | | |
+ | |110°C/60” |
− | | |
+ | |AZ300MIF |
− | | |
+ | |60" |
− | | align="left" | |
+ | | align="left" | |
− | *0.5 um isolated lines |
+ | *0.5 um isolated lines |
*{{fl|SPR955CMstepperrecipe.pdf|See SPR955CM data file}} |
*{{fl|SPR955CMstepperrecipe.pdf|See SPR955CM data file}} |
||
|- |
|- |
||
− | | |
+ | |SPR955CM0.9 |
− | | |
+ | |3 krpm/30” |
− | | |
+ | |95°C/60” |
− | | |
+ | |~ 0.9 um |
− | | |
+ | |3.0” |
− | | |
+ | |4 |
− | | |
+ | |110°C/60” |
− | | |
+ | |AZ300MIF |
− | | |
+ | |60" |
− | | align="left" | |
+ | | align="left" | |
− | *0.5 um |
+ | *0.5 um holes |
− | *Much longer exposure time for dense isolated holes |
+ | *Much longer exposure time for dense isolated holes |
*{{fl|SPR955CMstepperrecipe.pdf|See SPR955CM data file}} |
*{{fl|SPR955CMstepperrecipe.pdf|See SPR955CM data file}} |
||
|- |
|- |
||
− | | |
+ | |SPR955CM0.9<br> |
CEM365iS |
CEM365iS |
||
+ | |3 krpm/30”<br> |
||
− | |||
− | | 3 krpm/30”<br> |
||
5 krpm/30” |
5 krpm/30” |
||
+ | |95°C/90” |
||
− | |||
+ | |~ 0.9 um |
||
− | | 95°C/90” |
||
+ | |2.2” |
||
− | | ~ 0.9 um |
||
− | | |
+ | | -10 |
+ | |110°C/60” |
||
− | | -10 |
||
+ | |AZ300MIF |
||
− | | 110°C/60” |
||
+ | |60" |
||
− | | AZ300MIF |
||
− | | |
+ | | align="left" | |
+ | *0.35um isolated spaces by SEM measurement. |
||
− | | align="left" | |
||
+ | *Higher exposure time due to CEM |
||
− | *0.35um isolated spaces by SEM measurement. |
||
− | *Higher exposure time due to CEM |
||
*{{fl|SPR955CMstepperrecipe.pdf|See SPR955CM data file}} |
*{{fl|SPR955CMstepperrecipe.pdf|See SPR955CM data file}} |
||
|- |
|- |
||
− | | |
+ | |SPR950-0.8 |
− | | |
+ | |4 krpm/30” |
− | | |
+ | |95°C/60” |
− | | |
+ | |~ 0.8 um |
− | | |
+ | |1.0” |
− | | |
+ | |0 |
− | | |
+ | |105°C/60” |
− | | |
+ | |AZ300MIF |
− | | |
+ | |60" |
− | | align="left" | |
+ | | align="left" | |
+ | |||
|- |
|- |
||
− | | |
+ | |SPR955CM-1.8 |
− | | |
+ | |4 krpm/30” |
− | | |
+ | |90°C/90” |
− | | |
+ | |~ 1.8 um |
− | | |
+ | |2.3” |
− | | |
+ | |0 |
− | | |
+ | |110°C/90” |
− | | |
+ | |AZ300MIF |
− | | |
+ | |60" |
− | | align="left" | |
+ | | align="left" | |
− | *0.5 um isolated lines |
+ | *0.5 um isolated lines |
*{{fl|spr955_1.8GCA6300.pdf|See 955CM-1.8 data file}} |
*{{fl|spr955_1.8GCA6300.pdf|See 955CM-1.8 data file}} |
||
|- |
|- |
||
− | | |
+ | |SPR955CM-1.8 |
− | | |
+ | |4 krpm/30” |
− | | |
+ | |90°C/90” |
− | | |
+ | |~ 1.8 um |
− | | |
+ | |1.7” |
− | | |
+ | | -5 |
− | | |
+ | |110°C/90” |
− | | |
+ | |AZ300MIF |
− | | |
+ | |60" |
− | | align="left" | |
+ | | align="left" | |
− | * |
+ | *1 um isolated posts |
+ | *{{fl|spr955_1.8GCA6300.pdf|See 955CM-1.8 data file}} |
||
+ | |||
+ | |- |
||
+ | |SPR220-3.0 |
||
+ | |2.5 krpm/30” |
||
+ | |115°C/90” |
||
+ | |~ 2.7 um |
||
+ | |2.4” |
||
+ | |10 |
||
+ | |115°C/90” |
||
+ | |AZ300MIF |
||
+ | |60" |
||
+ | | align="left" | |
||
+ | *0.5 um isolated lines |
||
*{{fl|SPR-220-3.0_OptimizationNew.pdf|See SPR220-3 Data File}} |
*{{fl|SPR-220-3.0_OptimizationNew.pdf|See SPR220-3 Data File}} |
||
|- |
|- |
||
− | | |
+ | |SPR220-7.0 |
− | | |
+ | |3.5 krpm/45” |
− | | |
+ | |115°C/120” |
− | | |
+ | |~ 7.0 um |
− | | |
+ | |4.5” |
− | | |
+ | |0 |
− | | |
+ | |*50°C/60”<br> |
115°C/90” |
115°C/90” |
||
− | | |
+ | |AZ300MIF |
− | | |
+ | |120" |
− | | align="left" | |
+ | | align="left" | |
*1.0 um isolated lines; 1.25 um isolated spaces |
*1.0 um isolated lines; 1.25 um isolated spaces |
||
− | **Let sample sit in air for 20 minutes before PEB, step to 50°C for 60” first, then 115°C |
+ | **Let sample sit in air for 20 minutes before PEB, step to 50°C for 60” first, then 115°C |
*{{fl|SPR-220-7.0stepperrecipe.pdf|See SPR220-7 Data File}} |
*{{fl|SPR-220-7.0stepperrecipe.pdf|See SPR220-7 Data File}} |
||
Line 133: | Line 154: | ||
Unless otherwise noted, bakes are on hot plate. All flood exposures are done in broadband light using any contact aligner. Also, because the tone is negative, a shorter first exposure time will result in more undercut, which is desirable for single-layer lift-off processes. Under these conditions more develop time will also give more undercut. |
Unless otherwise noted, bakes are on hot plate. All flood exposures are done in broadband light using any contact aligner. Also, because the tone is negative, a shorter first exposure time will result in more undercut, which is desirable for single-layer lift-off processes. Under these conditions more develop time will also give more undercut. |
||
− | {| |
+ | {| class="wikitable" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center;" border="1" |
|- bgcolor="#D0E7FF" |
|- bgcolor="#D0E7FF" |
||
− | ! width="100" | |
+ | ! width="100" |Resist |
− | ! width="100" | |
+ | ! width="100" |Spin Cond. |
− | ! width="75" | |
+ | ! width="75" |Bake |
− | ! width="75" | |
+ | ! width="75" |Thickness |
− | ! width="125" | |
+ | ! width="125" |Exposure Time |
− | ! width="100" | |
+ | ! width="100" |Focus Offset |
− | ! width="75" | |
+ | ! width="75" |PEB |
− | ! width="75" | |
+ | ! width="75" |Flood |
− | ! width="100" | |
+ | ! width="100" |Developer |
− | ! width="125" | |
+ | ! width="125" |Developer Time |
− | ! width="300" | |
+ | ! width="300" |Comments |
|- |
|- |
||
− | | |
+ | |AZ5214 |
− | | |
+ | |6 krpm/30” |
− | | |
+ | |95°C/60” |
− | | |
+ | |~ 1.0 um |
− | | |
+ | |0.2” |
− | | |
+ | |0 |
− | | |
+ | |110°C/60” |
− | | |
+ | |60" |
− | | |
+ | |AZ300MIF |
− | | |
+ | |60" |
− | | align="left" | |
+ | | align="left" | |
*0.7 um res. possible |
*0.7 um res. possible |
||
|- |
|- |
||
− | | |
+ | |nLOF5510 |
− | | |
+ | |3 krpm/30” |
− | | |
+ | |90°C/60” |
− | | |
+ | |~ 0.93 um |
− | | |
+ | |0.74” |
− | | -6 |
+ | | -6 |
− | | |
+ | |110°C/60” |
− | | |
+ | |0 |
− | | |
+ | |AZ300MIF |
− | | |
+ | |60" |
− | | align="left" | |
+ | | align="left" | |
− | *0.5 um line openings good dense or isolated |
+ | *0.5 um line openings good dense or isolated |
− | *Use heated 1165 stripper for removal or lift-off |
+ | *Use heated 1165 stripper for removal or lift-off |
*{{fl|nLOF5510stepperrecipe.pdf|See nLOF5510 data file}} |
*{{fl|nLOF5510stepperrecipe.pdf|See nLOF5510 data file}} |
||
|- |
|- |
||
− | | |
+ | |nLOF2020 |
− | | |
+ | |4 krpm/30” |
− | | |
+ | |110°C/60” |
− | | |
+ | |~ 2 um |
− | | |
+ | |0.55” |
− | | -6 |
+ | | -6 |
− | | |
+ | |110°C/60” |
− | | |
+ | |0 |
− | | |
+ | |AZ300MIF |
− | | |
+ | |90" |
− | | align="left" | |
+ | | align="left" | |
− | *~ .85 um line opening/lift-off good. Isolated mesas can be smaller. |
+ | *~ .85 um line opening/lift-off good. Isolated mesas can be smaller. |
− | *Use heated 1165 stripper for removal or lift-off Sensetive to PEB temp. |
+ | *Use heated 1165 stripper for removal or lift-off Sensetive to PEB temp. |
*{{fl|nLOF2020stepperrecipe.pdf|See nLOF2020 Data File}} |
*{{fl|nLOF2020stepperrecipe.pdf|See nLOF2020 Data File}} |
||
|} |
|} |
||
− | = |
+ | =[[Stepper 2 (AutoStep 200)]]= |
==Positive Resist (AutoStep 200)== <!--Note that if this heading is changed, the recipe links on the Lithography page must be changed--> |
==Positive Resist (AutoStep 200)== <!--Note that if this heading is changed, the recipe links on the Lithography page must be changed--> |
||
Line 201: | Line 222: | ||
'''NOTE''': The bolded exposure times were found by multiplying the exposure times from the GCA 6300 system by 0.30. They should be sued as a starting point. You will need to do an exposure array to get precise times for the Autostep system. In general, the resolution achievable is ~ 100 nm smaller for the Autostep200 system. |
'''NOTE''': The bolded exposure times were found by multiplying the exposure times from the GCA 6300 system by 0.30. They should be sued as a starting point. You will need to do an exposure array to get precise times for the Autostep system. In general, the resolution achievable is ~ 100 nm smaller for the Autostep200 system. |
||
− | {| |
+ | {| class="wikitable" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center;" border="1" |
|- bgcolor="#D0E7FF" |
|- bgcolor="#D0E7FF" |
||
− | ! width="100" | |
+ | ! width="100" |Resist |
− | ! width="100" | |
+ | ! width="100" |Spin Cond. |
− | ! width="75" | |
+ | ! width="75" |Bake |
− | ! width="75" | |
+ | ! width="75" |Thickness |
− | ! width="125" | |
+ | ! width="125" |Exposure Time |
− | ! width="100" | |
+ | ! width="100" |Focus Offset |
− | ! width="75" | |
+ | ! width="75" |PEB |
− | ! width="100" | |
+ | ! width="100" |Developer |
− | ! width="125" | |
+ | ! width="125" |Developer Time |
− | ! width="300" | |
+ | ! width="300" |Comments |
|- |
|- |
||
− | | |
+ | |SPR955CM-0.9 |
− | | |
+ | |3 krpm/30” |
− | | |
+ | |95°C/90” |
− | | |
+ | |~ 0.9 um |
− | | |
+ | |0.35” |
− | | |
+ | |0 |
− | | |
+ | |110°C/90” |
− | | |
+ | |AZ300MIF |
− | | |
+ | |60” |
− | | align="left" | |
+ | | align="left" | |
− | *0.5um dense lines |
+ | *0.5um dense lines |
*{{fl|SPR955-0.9-AS200-stepperrecipe.pdf|See SPR955CM AS200 data file}} |
*{{fl|SPR955-0.9-AS200-stepperrecipe.pdf|See SPR955CM AS200 data file}} |
||
|- |
|- |
||
− | | |
+ | |SPR955CM-0.9 |
− | | |
+ | |3 krpm/30” |
− | | |
+ | |95°C/90” |
− | | |
+ | |~ 0.9 um |
− | | |
+ | |0.8” |
− | | |
+ | |0 |
− | | |
+ | |110°C/90” |
− | | |
+ | |AZ300MIF |
− | | |
+ | |60” |
− | | align="left" | |
+ | | align="left" | |
*0.5um holes |
*0.5um holes |
||
|- |
|- |
||
− | | |
+ | |SPR955CM-1.8 |
− | | |
+ | |4 krpm/30” |
− | | |
+ | |95°C/90” |
− | | |
+ | |~ 1.8 um |
− | | |
+ | |0.4” |
− | | -1 |
+ | | -1 |
− | | |
+ | |110°C/90” |
− | | |
+ | |AZ300MIF |
− | | |
+ | |60” |
− | | align="left" | |
+ | | align="left" | |
*{{fl|SPR955-1.8-AS200-stepperrecipe.pdf|See SPR955-1.8 AS200 data file}} |
*{{fl|SPR955-1.8-AS200-stepperrecipe.pdf|See SPR955-1.8 AS200 data file}} |
||
|- |
|- |
||
− | | |
+ | |SPR950-0.8 |
− | | |
+ | |4 krpm/30” |
− | | |
+ | |95°C/60” |
− | | |
+ | |~ 0.8 um |
− | | |
+ | |'''0.30”''' |
− | | |
+ | |0 |
− | | |
+ | |105°C/60” |
− | | |
+ | |AZ300MIF |
− | | |
+ | |60" |
− | | align="left" | |
+ | | align="left" | |
|- |
|- |
||
− | | |
+ | |SPR220-3.0 |
− | | |
+ | |2.5 krpm/30” |
− | | |
+ | |115°C/90” |
− | | |
+ | |~ 2.7 um |
− | | |
+ | |'''0.72”''' |
− | | |
+ | |10 |
− | | |
+ | |115°C/90” |
− | | |
+ | |AZ300MIF |
− | | |
+ | |60" |
− | | align="left" | |
+ | | align="left" | |
*0.5 um isolated lines |
*0.5 um isolated lines |
||
|- |
|- |
||
− | | |
+ | |SPR220-7.0 |
− | | |
+ | |3.5 krpm/45” |
− | | |
+ | |115°C/120” |
− | | |
+ | |~ 7.0 um |
− | | |
+ | |'''1.35"''' |
− | | |
+ | |0 |
− | | |
+ | |*50°C/60”<br> |
115°C/90” |
115°C/90” |
||
− | | |
+ | |AZ300MIF |
− | | |
+ | |120" |
− | | align="left" | |
+ | | align="left" | |
*1.0 um isolated lines; 1.25 um isolated spaces |
*1.0 um isolated lines; 1.25 um isolated spaces |
||
**Let sample sit in air for 20 minutes before PEB, step to 50°C for 60” first, then 115°C |
**Let sample sit in air for 20 minutes before PEB, step to 50°C for 60” first, then 115°C |
||
+ | |||
+ | |- |
||
+ | |AZ4210 |
||
+ | |step1:500rpm/5", step2:4krpm/45” |
||
+ | |95°C/60" |
||
+ | |~ 2.1 um |
||
+ | |'''0.75"''' |
||
+ | |0 |
||
+ | | |
||
+ | |||
+ | |AZ400K:DI=1:4 |
||
+ | |60" |
||
+ | | align="left" | |
||
+ | *2.0 um dense holes |
||
|} |
|} |
||
Line 300: | Line 335: | ||
'''NOTE''': The bolded exposure times were found by multiplying the exposure times from the GCA 6300 system by 0.30. They should be sued as a starting point. You will need to do an exposure array to get precise times for the Autostep system. In general, the resolution achievable is ~ 100 nm smaller for the Autostep200 system. |
'''NOTE''': The bolded exposure times were found by multiplying the exposure times from the GCA 6300 system by 0.30. They should be sued as a starting point. You will need to do an exposure array to get precise times for the Autostep system. In general, the resolution achievable is ~ 100 nm smaller for the Autostep200 system. |
||
− | {| |
+ | {| class="wikitable" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center;" border="1" |
|- bgcolor="#D0E7FF" |
|- bgcolor="#D0E7FF" |
||
− | ! width="100" | |
+ | ! width="100" |Resist |
− | ! width="100" | |
+ | ! width="100" |Spin Cond. |
− | ! width="75" | |
+ | ! width="75" |Bake |
− | ! width="75" | |
+ | ! width="75" |Thickness |
− | ! width="125" | |
+ | ! width="125" |Exposure Time |
− | ! width="100" | |
+ | ! width="100" |Focus Offset |
− | ! width="75" | |
+ | ! width="75" |PEB |
− | ! width="75" | |
+ | ! width="75" |Flood |
− | ! width="100" | |
+ | ! width="100" |Developer |
− | ! width="125" | |
+ | ! width="125" |Developer Time |
− | ! width="300" | |
+ | ! width="300" |Comments |
|- |
|- |
||
− | | |
+ | |nLOF5510 |
− | | |
+ | |3 krpm/30” |
− | | |
+ | |90°C/60” |
− | | |
+ | |~ 0.93 um |
− | | |
+ | |.25” |
− | | -1 |
+ | | -1 |
− | | |
+ | |110°C/60” |
− | | |
+ | |0 |
− | | |
+ | |AZ300MIF |
− | | |
+ | |60” |
− | | align="left" | |
+ | | align="left" | |
− | *0.4 um lines dense good |
+ | *0.4 um lines dense good |
− | *Use heated 1165 stripper for removal or lift-off |
+ | *Use heated 1165 stripper for removal or lift-off |
*{{fl|nLOF5510-AS200-stepperrecipe.pdf|See nLOF5510 As200 data file}} |
*{{fl|nLOF5510-AS200-stepperrecipe.pdf|See nLOF5510 As200 data file}} |
||
|- |
|- |
||
− | | |
+ | |AZ5214 |
− | | |
+ | |6 krpm/30” |
− | | |
+ | |95°C/60” |
− | | |
+ | |~ 1.0 um |
− | | |
+ | |'''0.06”''' |
− | | |
+ | |0 |
− | | |
+ | |110°C/60” |
− | | |
+ | |60" |
− | | |
+ | |AZ300MIF |
− | | |
+ | |60" |
− | | align="left" | |
+ | | align="left" | |
*0.7 um res. possible |
*0.7 um res. possible |
||
|- |
|- |
||
− | | |
+ | |nLOF2020 |
− | | |
+ | |4 krpm/30” |
− | | |
+ | |110°C/60” |
− | | |
+ | |~ 2 um |
− | | |
+ | |'''0.17”''' |
− | | -6 |
+ | | -6 |
− | | |
+ | |110°C/60” |
− | | |
+ | |0 |
− | | |
+ | |AZ300MIF |
− | | |
+ | |90" |
− | | align="left" | |
+ | | align="left" | |
− | *~ .85 um line opening/lift-off good. Isolated mesas can be smaller. |
+ | *~ .85 um line opening/lift-off good. Isolated mesas can be smaller. |
*Use heated 1165 stripper for removal or lift-off Sensetive to PEB temp. |
*Use heated 1165 stripper for removal or lift-off Sensetive to PEB temp. |
||
+ | |- |
||
+ | |NR9-1000PY |
||
+ | |3 krpm/30” |
||
+ | |135°C/180” lid down |
||
+ | |~ 1.2 um |
||
+ | |'''0.92”''' |
||
+ | |0 |
||
+ | |115°C/120” lid down |
||
+ | |0 |
||
+ | |AZ300MIF |
||
+ | |20" |
||
+ | | align="left" | |
||
+ | *~ .55 um line opening/lift-off good. |
||
+ | *Use heated 1165 stripper for removal 8Hrs min. |
||
+ | *{{fl|NR9-1000PY-AS200-stepperrecipe.pdf|See NR9-1000PY As200 data file}} |
||
|} |
|} |
||
− | = |
+ | =[[Stepper 3 (ASML DUV)]]= |
+ | |||
+ | ==Anti-Reflective Coatings== |
||
+ | Bottom Anti-reflective coatings (aka. BARC or AR Coating) are, in general, used for the ASML stepper. LOL2000 and PMGI can also be used as under layers. |
||
+ | |||
+ | ==='''[https://wiki.nanotech.ucsb.edu/wiki/images/0/07/DUV42P-Anti-Reflective-Coating.pdf DUV-42P-6]'''=== |
||
+ | ''(replacement for AR2)'' |
||
+ | |||
+ | *spin coat at 2500rpm for optimal anti-reflective properties (~60nm). |
||
+ | **Mistake: this was previously written as 3500rpm. |
||
+ | *Bake at 220°C for 60s on a hotplate. |
||
+ | *This AR coating is removed via oxygen plasma. |
||
+ | *This ARC can be etched on [https://wiki.nanotech.ucsb.edu/wiki/index.php/ICP_Etching_Recipes#Photoresist_and_ARC_Etching_.28Panasonic_1.29 ICP#1], [https://wiki.nanotech.ucsb.edu/wiki/index.php/ICP_Etching_Recipes#Photoresist_and_ARC_etching_.28Panasonic_2.29 ICP#2], [https://wiki.nanotech.ucsb.edu/wiki/index.php/RIE_Etching_Recipes#Photoresist_and_ARC_.28RIE_5.29 RIE#5], [https://wiki.nanotech.ucsb.edu/wiki/ICP_Etching_Recipes#Photoresist_.26_ARC_.28Fluorine_ICP_Etcher.29 FL-ICP] or even [[Ashers (Technics PEII)|Technics PEii ashers]]. |
||
+ | *Datasheet: '''[https://wiki.nanotech.ucsb.edu/wiki/images/0/07/DUV42P-Anti-Reflective-Coating.pdf DUV-42P-6]''' |
||
+ | |||
+ | ==='''[https://wiki.nanotech.ucsb.edu/wiki/images/a/af/DS-K101-304-Anti-Reflective-Coating.pdf DS-K101-304]'''=== |
||
+ | |||
+ | *spin at 5000rpm and bake at 185C for 60s. |
||
+ | **~20nm thickness |
||
+ | *This AR coating develops away and undercuts in AZ300MIF. |
||
+ | **For isolated lines, this can cause them to lift-off by undercutting the resist. |
||
+ | *Increase bake temperature to reduce undercut rate. |
||
+ | **[[DS-K101-304 Bake Temp. versus Develop Rate]] - Click for experimental data |
||
+ | **Can be used similarly to DUV42P (dry etch removal) by baking at 220°C. |
||
+ | *Datasheet: '''[https://wiki.nanotech.ucsb.edu/wiki/images/a/af/DS-K101-304-Anti-Reflective-Coating.pdf DS-K101-304]''' |
||
==Positive Resist (ASML DUV)== |
==Positive Resist (ASML DUV)== |
||
+ | Please see section above for anti-reflection coatings, which are usually used with the DUV Stepper. |
||
− | Anti-reflective coatings are, in general, used for the ASML stepper<span style="line-height: 1.5em;">. LOL2000 and PMGI</span><span style="line-height: 1.5em;"> can also be used. For AR2 coatings, spin coat at 3500rpm for a 670A thick coating. Bake at 220C for 60s on a hotplate. This AR coating is removed via oxygen plasma. RIE 5 parameters are 20sccm, 10mT, 100W for 40s. For DS-K101, spin at 5000rpm and bake at 185C for 60s. This AR coating develops away and undercuts in AZ300MIF. For isolated lines, this can cause them to lift-off. If undercut rate is too high, increase bake temperature. </span> |
||
− | {| |
+ | {| class="wikitable" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center;" border="1" |
|- bgcolor="#D0E7FF" |
|- bgcolor="#D0E7FF" |
||
− | ! width="100" | |
+ | ! width="100" |Resist |
− | ! width="100" | |
+ | ! width="100" |Spin Cond. |
− | ! width="75" | |
+ | ! width="75" |Bake |
− | ! width="75" | |
+ | ! width="75" |Thickness |
− | ! width="125" | |
+ | ! width="125" |Exposure Dose(mj) |
− | ! width="100" | |
+ | ! width="100" |Focus Offset |
− | ! width="75" | |
+ | ! width="75" |PEB |
− | ! width="100" | |
+ | ! width="100" |Developer |
− | ! width="125" | |
+ | ! width="125" |Developer Time |
− | ! width="300" | |
+ | ! width="300" |Comments |
|- |
|- |
||
− | | |
+ | |UV6-0.7 <br> (replaced by UV6-0.8) |
+ | |||
− | | 3.5 krpm/30” |
||
+ | |3.5 krpm/30” |
||
− | | 135°C/60” |
||
+ | |135°C/60” |
||
− | | 630nm |
||
+ | |630nm |
||
− | | 17 |
||
+ | |17 |
||
− | | -0.2 |
||
+ | | -0.2 |
||
− | | 135°C/90” |
||
+ | |135°C/90” |
||
− | | AZ300MIF |
||
+ | |AZ300MIF |
||
− | | 45” |
||
+ | |45” |
||
− | | align="left" | |
||
+ | | align="left" | |
||
− | *200nm dense line/space |
||
+ | *200nm dense line/space |
||
− | *NA 0.57, Sigma 0.75 |
||
+ | *NA 0.57, Sigma 0.75 |
||
*Eo ~ 5.5mj |
*Eo ~ 5.5mj |
||
+ | *UV6-0.7 was discontinued, we now stock UV6-0.8 |
||
|- |
|- |
||
− | | |
+ | |UV210-0.3 |
− | | |
+ | |5.0 krpm/30” |
− | | |
+ | |135°C/60” |
− | | |
+ | |230nm |
− | | |
+ | |20 |
− | | -0.1 |
+ | | -0.1 |
− | | |
+ | |135°C/90” |
− | | |
+ | |AZ300MIF |
− | | |
+ | |45" |
− | | align="left" | |
+ | | align="left" | |
− | *150nm dense line/space |
+ | *150nm dense line/space |
+ | *'''Annular Illumination''' |
||
*NA 0.63, Sigma_o 0.8, Sigma_i 0.5 |
*NA 0.63, Sigma_o 0.8, Sigma_i 0.5 |
||
|- |
|- |
||
− | | |
+ | |UV210-0.3 |
− | | |
+ | |3.0 krpm/30” |
− | | |
+ | |135°C/90” |
− | | |
+ | |260nm |
− | | |
+ | |85 |
− | | -0.2 |
+ | | -0.2 |
− | | |
+ | |135°C/90” |
− | | |
+ | |AZ300MIF |
− | | |
+ | |80” |
− | | align="left" | |
+ | | align="left" | |
− | *170nm isolated holes |
+ | *170nm isolated holes |
+ | *'''Annular Illumination''' |
||
*NA 0.63, Sigma_o 0.8, Sigma_i 0.5 |
*NA 0.63, Sigma_o 0.8, Sigma_i 0.5 |
||
|} |
|} |
||
− | ==Negative Resist ( |
+ | ==Negative Resist (ASML DUV)== |
+ | Please see section above for anti-reflection coatings, which are usually used with the DUV Stepper. |
||
− | <span style="line-height: 1.5em;">Anti-reflective coatings are, in general, used for the ASML stepper. LOL2000 and PMGI can also be used. For AR2 coatings, spin coat at 3500rpm for a 670A thick coating. Bake at 220C for 60s on a hotplate. This AR coating is removed via oxygen plasma. RIE 5 parameters are 20sccm, 10mT, 100W for 40s. For DS-K101, spin at 5000rpm and bake at 185C for 60s. This AR coating develops away and undercuts in AZ300MIF. For isolated lines, this can cause them to lift-off. If undercut rate is too high, increase bake temperature.</span> |
||
+ | {| class="wikitable" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center;" border="1" |
||
− | <br> |
||
− | |||
− | {| border="1" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center;" class="wikitable" |
||
|- bgcolor="#D0E7FF" |
|- bgcolor="#D0E7FF" |
||
− | ! width="100" | |
+ | ! width="100" |Resist |
− | ! width="100" | |
+ | ! width="100" |Spin Cond. |
− | ! width="75" | |
+ | ! width="75" |Bake |
− | ! width="75" | |
+ | ! width="75" |Thickness |
− | ! width="125" | |
+ | ! width="125" |Exposure Dose (mj) |
− | ! width="100" | |
+ | ! width="100" |Focus Offset |
− | ! width="75" | |
+ | ! width="75" |PEB |
− | ! width="75" | |
+ | ! width="75" |Flood |
− | ! width="100" | |
+ | ! width="100" |Developer |
− | ! width="125" | |
+ | ! width="125" |Developer Time |
− | ! width="300" | |
+ | ! width="300" |Comments |
|- |
|- |
||
− | | |
+ | |UVN30-0.8 |
− | | |
+ | |3.5 krpm/30” |
− | | |
+ | |110°C/60” |
− | | |
+ | |~550nm |
+ | |27 |
||
− | | 23 |
||
− | | +0. |
+ | | +0.15 |
− | | |
+ | |105°C/60” |
− | | |
+ | |Not Used |
− | | |
+ | |AZ300MIF |
+ | |55-60 sec |
||
− | | 40” |
||
− | | align="left" | |
+ | | align="left" | |
+ | *Replaced UVN2300, not identical |
||
− | *200nm isolated line |
||
− | *NA 0.57, Sigma 0.5 |
||
|} |
|} |
||
+ | |||
+ | == Other Lithography Processes (ASML DUV) == |
||
+ | * [[ASML DUV: Edge Bead Removal via Photolithography|DUV Photolithographic Edge Bead Removal]] |
||
+ | * [[Lift-Off with DUV Imaging + PMGI Underlayer|DUV Lift-Off Process with PMGI Underlayer]] |
Revision as of 10:58, 27 July 2021
Back to Lithography Recipes.
Below is a listing of stepper lithography recipes. Stepper 1 and Stepper 2 are i-line systems with good piece handling capabilities. Stepper 3 is a DUV (248nm) system primarily used for full 100mm wafers. DUV resists do not work for i-line and i-line resists do not work for DUV. Based on your sample reflectivity, absorption (or whether or not you use an ARC layer), and surface topography, the exposure time / focus offset parameters may vary.
This listing is a guideline to get you started. For critical lithography steps, you should run your own exposure and/or focus array to determine the proper parameters.
The recipes are tabulated to give you the values of the key parameters you will need to establish your recipe. Underlayers such as LOL2000 or PMGI can be used on the stepper systems. See the underlayer datasheets for details. Post develop bakes (not listed) are used to make the resist more etch resistant and depend on subsequent processes. Care should be taken with post development bakes as resist reflow can occur. Unless otherwise noted, all exposures are done on flat, silicon wafers.
Parameters are indicated in separate tables for each stepper system.
Stepper 1 (GCA 6300)
Multiply the GCA 6300 exposure times by 0.30 to get a starting exposure time for the GCA Autostep200 system.
Positive Resist (GCA 6300)
Unless otherwise noted, bakes are on hot plates. For recipes with CEM, the CEM is spun on after the first resist bake, exposure is then done, and the CEM is rinsed off with DI water before the PEB. CEM generally improves resolution and process tolerance at the expense of higher exposure time.
Resist | Spin Cond. | Bake | Thickness | Exposure Time | Focus Offset | PEB | Developer | Developer Time | Comments |
---|---|---|---|---|---|---|---|---|---|
SPR955CM0.9 | 3 krpm/30” | 95°C/60” | ~ 0.9 um | 1.2” | 0 | 110°C/60” | AZ300MIF | 60" |
|
SPR955CM0.9 | 3 krpm/30” | 95°C/60” | ~ 0.9 um | 3.0” | 4 | 110°C/60” | AZ300MIF | 60" |
|
SPR955CM0.9 CEM365iS |
3 krpm/30” 5 krpm/30” |
95°C/90” | ~ 0.9 um | 2.2” | -10 | 110°C/60” | AZ300MIF | 60" |
|
SPR950-0.8 | 4 krpm/30” | 95°C/60” | ~ 0.8 um | 1.0” | 0 | 105°C/60” | AZ300MIF | 60" | |
SPR955CM-1.8 | 4 krpm/30” | 90°C/90” | ~ 1.8 um | 2.3” | 0 | 110°C/90” | AZ300MIF | 60" |
|
SPR955CM-1.8 | 4 krpm/30” | 90°C/90” | ~ 1.8 um | 1.7” | -5 | 110°C/90” | AZ300MIF | 60" |
|
SPR220-3.0 | 2.5 krpm/30” | 115°C/90” | ~ 2.7 um | 2.4” | 10 | 115°C/90” | AZ300MIF | 60" |
|
SPR220-7.0 | 3.5 krpm/45” | 115°C/120” | ~ 7.0 um | 4.5” | 0 | *50°C/60” 115°C/90” |
AZ300MIF | 120" |
|
Negative Resist (GCA 6300)
Unless otherwise noted, bakes are on hot plate. All flood exposures are done in broadband light using any contact aligner. Also, because the tone is negative, a shorter first exposure time will result in more undercut, which is desirable for single-layer lift-off processes. Under these conditions more develop time will also give more undercut.
Resist | Spin Cond. | Bake | Thickness | Exposure Time | Focus Offset | PEB | Flood | Developer | Developer Time | Comments |
---|---|---|---|---|---|---|---|---|---|---|
AZ5214 | 6 krpm/30” | 95°C/60” | ~ 1.0 um | 0.2” | 0 | 110°C/60” | 60" | AZ300MIF | 60" |
|
nLOF5510 | 3 krpm/30” | 90°C/60” | ~ 0.93 um | 0.74” | -6 | 110°C/60” | 0 | AZ300MIF | 60" |
|
nLOF2020 | 4 krpm/30” | 110°C/60” | ~ 2 um | 0.55” | -6 | 110°C/60” | 0 | AZ300MIF | 90" |
|
Stepper 2 (AutoStep 200)
Positive Resist (AutoStep 200)
Unless otherwise noted, bakes are on hot plates. For recipes with CEM, the CEM is spun on after the first resist bake, exposure is then done, and the CEM is rinsed off with DI water before the PEB. CEM generally improves resolution and process tolerance at the expense of higher exposure time.
NOTE: The bolded exposure times were found by multiplying the exposure times from the GCA 6300 system by 0.30. They should be sued as a starting point. You will need to do an exposure array to get precise times for the Autostep system. In general, the resolution achievable is ~ 100 nm smaller for the Autostep200 system.
Resist | Spin Cond. | Bake | Thickness | Exposure Time | Focus Offset | PEB | Developer | Developer Time | Comments |
---|---|---|---|---|---|---|---|---|---|
SPR955CM-0.9 | 3 krpm/30” | 95°C/90” | ~ 0.9 um | 0.35” | 0 | 110°C/90” | AZ300MIF | 60” |
|
SPR955CM-0.9 | 3 krpm/30” | 95°C/90” | ~ 0.9 um | 0.8” | 0 | 110°C/90” | AZ300MIF | 60” |
|
SPR955CM-1.8 | 4 krpm/30” | 95°C/90” | ~ 1.8 um | 0.4” | -1 | 110°C/90” | AZ300MIF | 60” | |
SPR950-0.8 | 4 krpm/30” | 95°C/60” | ~ 0.8 um | 0.30” | 0 | 105°C/60” | AZ300MIF | 60" | |
SPR220-3.0 | 2.5 krpm/30” | 115°C/90” | ~ 2.7 um | 0.72” | 10 | 115°C/90” | AZ300MIF | 60" |
|
SPR220-7.0 | 3.5 krpm/45” | 115°C/120” | ~ 7.0 um | 1.35" | 0 | *50°C/60” 115°C/90” |
AZ300MIF | 120" |
|
AZ4210 | step1:500rpm/5", step2:4krpm/45” | 95°C/60" | ~ 2.1 um | 0.75" | 0 | AZ400K:DI=1:4 | 60" |
|
Negative Resist (AutoStep 200)
Unless otherwise noted, bakes are on hot plate. All flood exposures are done in broadband light using any contact aligner. Also, because the tone is negative, a shorter first exposure time will result in more undercut, which is desirable for single-layer lift-off processes. Under these conditions more develop time will also give more undercut.
NOTE: The bolded exposure times were found by multiplying the exposure times from the GCA 6300 system by 0.30. They should be sued as a starting point. You will need to do an exposure array to get precise times for the Autostep system. In general, the resolution achievable is ~ 100 nm smaller for the Autostep200 system.
Resist | Spin Cond. | Bake | Thickness | Exposure Time | Focus Offset | PEB | Flood | Developer | Developer Time | Comments |
---|---|---|---|---|---|---|---|---|---|---|
nLOF5510 | 3 krpm/30” | 90°C/60” | ~ 0.93 um | .25” | -1 | 110°C/60” | 0 | AZ300MIF | 60” |
|
AZ5214 | 6 krpm/30” | 95°C/60” | ~ 1.0 um | 0.06” | 0 | 110°C/60” | 60" | AZ300MIF | 60" |
|
nLOF2020 | 4 krpm/30” | 110°C/60” | ~ 2 um | 0.17” | -6 | 110°C/60” | 0 | AZ300MIF | 90" |
|
NR9-1000PY | 3 krpm/30” | 135°C/180” lid down | ~ 1.2 um | 0.92” | 0 | 115°C/120” lid down | 0 | AZ300MIF | 20" |
|
Stepper 3 (ASML DUV)
Anti-Reflective Coatings
Bottom Anti-reflective coatings (aka. BARC or AR Coating) are, in general, used for the ASML stepper. LOL2000 and PMGI can also be used as under layers.
DUV-42P-6
(replacement for AR2)
- spin coat at 2500rpm for optimal anti-reflective properties (~60nm).
- Mistake: this was previously written as 3500rpm.
- Bake at 220°C for 60s on a hotplate.
- This AR coating is removed via oxygen plasma.
- This ARC can be etched on ICP#1, ICP#2, RIE#5, FL-ICP or even Technics PEii ashers.
- Datasheet: DUV-42P-6
DS-K101-304
- spin at 5000rpm and bake at 185C for 60s.
- ~20nm thickness
- This AR coating develops away and undercuts in AZ300MIF.
- For isolated lines, this can cause them to lift-off by undercutting the resist.
- Increase bake temperature to reduce undercut rate.
- DS-K101-304 Bake Temp. versus Develop Rate - Click for experimental data
- Can be used similarly to DUV42P (dry etch removal) by baking at 220°C.
- Datasheet: DS-K101-304
Positive Resist (ASML DUV)
Please see section above for anti-reflection coatings, which are usually used with the DUV Stepper.
Resist | Spin Cond. | Bake | Thickness | Exposure Dose(mj) | Focus Offset | PEB | Developer | Developer Time | Comments |
---|---|---|---|---|---|---|---|---|---|
UV6-0.7 (replaced by UV6-0.8) |
3.5 krpm/30” | 135°C/60” | 630nm | 17 | -0.2 | 135°C/90” | AZ300MIF | 45” |
|
UV210-0.3 | 5.0 krpm/30” | 135°C/60” | 230nm | 20 | -0.1 | 135°C/90” | AZ300MIF | 45" |
|
UV210-0.3 | 3.0 krpm/30” | 135°C/90” | 260nm | 85 | -0.2 | 135°C/90” | AZ300MIF | 80” |
|
Negative Resist (ASML DUV)
Please see section above for anti-reflection coatings, which are usually used with the DUV Stepper.
Resist | Spin Cond. | Bake | Thickness | Exposure Dose (mj) | Focus Offset | PEB | Flood | Developer | Developer Time | Comments |
---|---|---|---|---|---|---|---|---|---|---|
UVN30-0.8 | 3.5 krpm/30” | 110°C/60” | ~550nm | 27 | +0.15 | 105°C/60” | Not Used | AZ300MIF | 55-60 sec |
|