Difference between revisions of "Sputtering Recipes"
(→Sputter 5 (Lesker AXXIS): link to SUM page for installed targets) |
(→Sputter 3 (AJA ATC 2000-F): Reduced Heading Levels below "Page Title") |
||
(20 intermediate revisions by 4 users not shown) | |||
Line 2: | Line 2: | ||
{{rl|Atomic Layer Deposition Recipes|Pt deposition (ALD)}} |
{{rl|Atomic Layer Deposition Recipes|Pt deposition (ALD)}} |
||
− | =[[Sputter |
+ | ==[[Sputter 3 (AJA ATC 2000-F)]]== |
− | == Al Deposition (Sputter 2) == |
||
− | *[[media:20-Al-Sputtering-Film-Sputter-2.pdf|Al Deposition Recipe]] |
||
− | == AlN<sub>x</sub> Deposition (Sputter 2) == |
||
− | *[[media:Sputter-2-AlN-Endeavor-rev1.pdf|AlN<sub>x</sub> Deposition Recipe]] |
||
+ | Please see the [https://signupmonkey.ece.ucsb.edu/cgi-bin/users/browse.cgi?tool_ID=20 SignupMonkey Page] for a list of currently installed targets. |
||
− | == Au Deposition (Sputter 2) == |
||
− | *[[media:21-Au-Sputter-film-recipes-Sputter-2.pdf|Au Deposition Recipe]] |
||
− | == TiO<sub>2</sub> Deposition (Sputter 2) == |
||
− | *[[media:22-TiO2-Film-Sputter-2.pdf|TiO2<sub>2</sub> Deposition Recipe]] |
||
− | |||
− | =[[Sputter 3 (AJA ATC 2000-F)]]= |
||
− | |||
− | The recipes below are given as starting points from data obtained in the nanofab. For critical depositions, calibrations are recommended. Please see the [https://signupmonkey.ece.ucsb.edu/cgi-bin/users/browse.cgi?tool_ID=20 SignupMonkey Page] for a list of currently installed targets. |
||
+ | === Materials Table (Sputter 3) === |
||
+ | The recipes below are given as starting points from data obtained in the nanofab. For critical depositions, calibrations are recommended. |
||
{| class="wikitable sortable" |
{| class="wikitable sortable" |
||
|- |
|- |
||
− | ! |
+ | !Material!!P(mT)!!Pow(W)!!Sub(W)!!T(C)!!Ar!!N2!!O2!!Height-Tilt!!Rate(nm/min)!!Stress(MPa)!!Rs(uOhm-cm)!!n@633nm!!k@633nm |
+ | !Target Consumed Lower Limit!!Data Below!!Comment |
||
+ | |- |
||
+ | |Au |
||
+ | | - |
||
+ | | - |
||
+ | | - |
||
+ | | - |
||
+ | | - |
||
+ | | - |
||
+ | | - |
||
+ | | - |
||
+ | | - |
||
+ | | - |
||
+ | | - |
||
+ | | - |
||
+ | | - |
||
+ | |Set: 200 W |
||
+ | Read: 400 VDC |
||
+ | |no |
||
+ | | |
||
|- |
|- |
||
|Al2O3 |
|Al2O3 |
||
Line 35: | Line 46: | ||
|1.6478 |
|1.6478 |
||
|0 |
|0 |
||
+ | | |
||
|no |
|no |
||
|Demis D. John |
|Demis D. John |
||
|- |
|- |
||
− | | |
+ | |Co||10(5)||200||0||20||25||0||0||25-9||2.3||-||-||-||- |
+ | | ||yes||Alex K |
||
|- |
|- |
||
− | | |
+ | |Cr||5||200||0||20||25||0||0||44-4||6.84||-||-||-||- |
+ | | ||no||Brian |
||
|- |
|- |
||
− | | |
+ | |Cu||1.5||50(395v)||0||20||25||0||0||25-9||4.15||-||-||-||- |
+ | | ||no||Ning |
||
|- |
|- |
||
− | | |
+ | |Cu||5||150(~490v)||0||20||15||0||0||0.82"-9||8||-||-||-||- |
+ | | ||yes||Ning |
||
|- |
|- |
||
− | | |
+ | |Fe||10(5)||200||0||20||25||0||0||25-9||1.25||-||-||-||- |
+ | | ||No||Alex K |
||
|- |
|- |
||
− | | |
+ | |Mo||3||200||0||20||25||0||0||44-4||13.15||-||-||-||- |
+ | | ||yes||Ning |
||
|- |
|- |
||
− | | |
+ | |Ni||5||150||0||20||25||0||0||44-4||5.23||-||-||-||- |
+ | | ||yes||Ning |
||
|- |
|- |
||
− | | |
+ | |Ni||5||150||0||20||25||0||0||25-9||1.82||-||-||-||- |
+ | | ||yes||Ning |
||
|- |
|- |
||
− | | |
+ | |Ni||5||75||0||20||25||0||0||44-4||2.50||-||-||-||- |
+ | | ||yes||Ning |
||
|- |
|- |
||
− | | |
+ | |Ni||3||200||0||20||25||0||0||44-4||9.4||-||-||-||- |
+ | | ||yes||Ning |
||
|- |
|- |
||
− | | |
+ | |Ni||1.5||50(399v)||0||20||25||0||0||25-9||0.96||-||-||-||- |
+ | | ||no||Ning |
||
|- |
|- |
||
− | | |
+ | |Pt||3||50||0||20||25||0||0||0.82"-9||2.9||-||-||-||- |
+ | | ||no||Ning |
||
|- |
|- |
||
− | | |
+ | |Si||8||250||0||25||25||0||0||15-3||1.4||-||-||-||- |
+ | | ||no||Gerhard - ramp 2W/s - 3% Unif 4" wafer |
||
|- |
|- |
||
− | | |
+ | |SiN||3||200||10||20||25||3||0||25-9||1.56||-||-||1.992||- |
+ | | ||yes||Brian |
||
|- |
|- |
||
− | | |
+ | |SiN||3||250||10||20||25||2.5||0||25-9||2.1||-||-||2.06||- |
+ | | ||yes||Brian |
||
|- |
|- |
||
− | | |
+ | |SiO2||3||200||10||20||25||0||3||25-9||3.68||-||-||1.447||- |
+ | | ||yes||Brian |
||
|- |
|- |
||
− | | |
+ | |SiO2||3||200||10||20||25||0||5||45-3||2.60||-||-||1.471||- |
+ | | ||yes||Brian |
||
|- |
|- |
||
− | | |
+ | |SiO2||3||250||10||20||25||0||2.5||25-9||4.3||-||-||1.485||- |
+ | | ||yes||Brian |
||
|- |
|- |
||
− | | |
+ | |Ta||5||150||0||20||25||0||0||44-4||9.47||-||-||-||- |
+ | | ||yes||Ning |
||
|- |
|- |
||
− | | |
+ | |Ta||5||75||0||20||25||0||0||44-4||5.03||-||-||-||- |
+ | | ||yes||Ning |
||
|- |
|- |
||
− | | |
+ | |Ti||3||100||0||20||25||0||0||25-9||1.34||-||-||-||- |
+ | | ||yes||Ning |
||
|- |
|- |
||
− | | |
+ | |SampleClean-NativeSiO2||10||0||18||20||25||0||0||44-4||-||-||-||-||- |
+ | | ||yes||150Volts 5 min |
||
|- |
|- |
||
|} |
|} |
||
− | == |
+ | ===Height Conversion for Older Recipes=== |
Old recipes using the manual Height setting in millimeters can be converted to the new programmatic settings in inches as follows: |
Old recipes using the manual Height setting in millimeters can be converted to the new programmatic settings in inches as follows: |
||
{| class="wikitable" |
{| class="wikitable" |
||
Line 105: | Line 139: | ||
Interpolation plot [[:File:Sputter 3 - height conversion v1.PNG|can be found here.]] |
Interpolation plot [[:File:Sputter 3 - height conversion v1.PNG|can be found here.]] |
||
− | == |
+ | ===Fe and Co Deposition (Sputter 3)=== |
− | *[[media:Fe and Co Films using Sputter-3.pdf|Fe and Co Deposition Recipe]] |
||
− | == Cu Deposition (Sputter 3) == |
||
− | *[[media:Cu Film using Sputter-3.pdf|Cu Deposition Recipe]] |
||
+ | *[//wiki.nanotech.ucsb.edu/wiki/images/1/15/Fe_and_Co_Films_using_Sputter-3.pdf Fe and Co Deposition Recipe] |
||
− | == Mo Deposition (Sputter 3) == |
||
− | *[[media:46-Mo Film using Sputter3.pdf|Mo Deposition Recipe]] |
||
− | == |
+ | ===Cu Deposition (Sputter 3)=== |
− | *[[media:24-Ni and Ta Films using Sputter-3.pdf|Ni and Ta Deposition Recipe]] |
||
− | *[[media:Ni Sputtering Film using Sputter 3-a.pdf|Ni Sputtering Film Recipe-3mT-200W]] |
||
+ | *[//wiki.nanotech.ucsb.edu/wiki/images/5/5e/Cu_Film_using_Sputter-3.pdf Cu Deposition Recipe] |
||
− | == SiO2 Deposition (Sputter 3) == |
||
− | *[[media:SiO2-AJA-1-Reactive-Sputter-Uniformity-rev-1.pdf|SiO2 Uniformity Data]] |
||
− | *[[media:SiO2-AJA-1-Reactive-Sputter-Power-Flow-AFM-Roughness-rev1.pdf|SiO2 Flow and Bias Variations Including AFM Data]] |
||
− | == |
+ | ===Mo Deposition (Sputter 3)=== |
− | *[[media:SiN-AJA-1-Reactive-Sputtering-Power-Flow-AFM-Rate-Index-rev1.pdf|SiN Flow and RF Variations Including AFM Data]] |
||
+ | *[//wiki.nanotech.ucsb.edu/wiki/images/7/7f/46-Mo_Film_using_Sputter3.pdf Mo Deposition Recipe] |
||
− | == Ti Deposition (Sputter 3) == |
||
− | *[[media:Ti Sputtering Film using Sputter 3.pdf|Ti Sputtering Film Recipe-3mT-100W]] |
||
+ | ===Ni and Ta Deposition (Sputter 3)=== |
||
− | =[[Sputter 4 (AJA ATC 2200-V)]]= |
||
+ | *[//wiki.nanotech.ucsb.edu/wiki/images/b/b6/24-Ni_and_Ta_Films_using_Sputter-3.pdf Ni and Ta Deposition Recipe] |
||
− | The recipes below are given as starting points from data obtained in the nanofab. For critical depositions, calibrations are recommended. Please see [https://signupmonkey.ece.ucsb.edu/cgi-bin/users/browse.cgi?tool_ID=21 the SignupMonkey page] for a list of currently installed targets. |
||
+ | *[//wiki.nanotech.ucsb.edu/wiki/images/9/93/Ni_Sputtering_Film_using_Sputter_3-a.pdf Ni Sputtering Film Recipe-3mT-200W] |
||
+ | ===SiO2 Deposition (Sputter 3)=== |
||
+ | |||
+ | *[//wiki.nanotech.ucsb.edu/wiki/images/e/ef/SiO2-AJA-1-Reactive-Sputter-Uniformity-rev-1.pdf SiO2 Uniformity Data] |
||
+ | *[//wiki.nanotech.ucsb.edu/wiki/images/b/b2/SiO2-AJA-1-Reactive-Sputter-Power-Flow-AFM-Roughness-rev1.pdf SiO2 Flow and Bias Variations Including AFM Data] |
||
+ | |||
+ | ===SiN Deposition (Sputter 3)=== |
||
+ | |||
+ | *[//wiki.nanotech.ucsb.edu/wiki/images/f/fb/SiN-AJA-1-Reactive-Sputtering-Power-Flow-AFM-Rate-Index-rev1.pdf SiN Flow and RF Variations Including AFM Data] |
||
+ | |||
+ | ===Ti Deposition (Sputter 3)=== |
||
+ | |||
+ | *[//wiki.nanotech.ucsb.edu/wiki/images/3/3b/Ti_Sputtering_Film_using_Sputter_3.pdf Ti Sputtering Film Recipe-3mT-100W] |
||
+ | |||
+ | ==[[Sputter 4 (AJA ATC 2200-V)]]== |
||
+ | |||
+ | Please see [https://signupmonkey.ece.ucsb.edu/cgi-bin/users/browse.cgi?tool_ID=21 the SignupMonkey page] for a list of currently installed targets. |
||
+ | |||
+ | === Materials Table (Sputter 4) === |
||
+ | The recipes below are given as starting points from data obtained in the nanofab. For critical depositions, calibrations are recommended. |
||
{| class="wikitable sortable" |
{| class="wikitable sortable" |
||
|- |
|- |
||
+ | !Material!!P(mT) |
||
− | ! Material !! P(mT) !! Pow(W) !! Sub(W) !! T(C) !! Ar !! N2 !! O2 !! Height-Tilt !! Rate(nm/min) !! Stress(MPa) !! Rs(uOhm-cm) !! n@633nm !! k@633nm !! Data Below !! Comment |
||
+ | !Power Source!!Pow(W)!!Sub(W)!!T(C)!!Ar!!N2!!O2!!Height-Tilt!!Rate(nm/min)!!Stress(MPa)!!Rs(uOhm-cm)!!n@633nm!!k@633nm!!Data Below!!Comment |
||
|- |
|- |
||
+ | |Al||5 |
||
− | | Al || 5 || 200 || 0 || 20 || 45 || 0 || 0 || H2.75-T5 || 4.4 || - || - || - || - || Yes || Ning Cao |
||
+ | | ||200||0||20||45||0||0||H2.75-T5||4.4||-||-||-||-||Yes||Ning Cao |
||
|- |
|- |
||
|Al2O3 |
|Al2O3 |
||
|3 |
|3 |
||
+ | |RF4-Sw1 |
||
|200 |
|200 |
||
− | (RF4-SW1) |
||
|0 |
|0 |
||
|20 |
|20 |
||
Line 155: | Line 201: | ||
|Demis D. John |
|Demis D. John |
||
|- |
|- |
||
+ | |Au||5 |
||
− | | Au || 5 || 200 || 0 || 20 || 45 || 0 || 0 || H1-T10 || 17.7 || - || - || - || - || Yes || Ning Cao |
||
+ | | ||200||0||20||45||0||0||H1-T10||17.7||-||-||-||-||Yes||Ning Cao |
||
|- |
|- |
||
+ | |Au||10 |
||
− | | Au || 10 || 300 || 0 || 20 || 45 || 0 || 0 || H2.75-T5 || 45.4 || - || - || - || - || Yes || Ning Cao |
||
+ | | ||300||0||20||45||0||0||H2.75-T5||45.4||-||-||-||-||Yes||Ning Cao |
||
|- |
|- |
||
+ | |Cu |
||
− | | Nb || 4 || 250 || 0 || 20 || 30 || 0 || 0 || H2.00-T7 || 7.5 || - || - || - || - || No || |
||
+ | |5 |
||
+ | | |
||
+ | |150 |
||
+ | |0 |
||
+ | |20 |
||
+ | |30 |
||
+ | |0 |
||
+ | |0 |
||
+ | |H0.82-T9 |
||
+ | |6.7 |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | |No (SEM available) |
||
+ | |Ning Cao |
||
|- |
|- |
||
+ | |Nb||4 |
||
− | | Pt || 5 || 200 || 0 || 20 || 45 || 0 || 0 || H2.75-T5 || 7.4 || - || - || - || - || Yes || Ning Cao |
||
+ | | ||250||0||20||30||0||0||H2.00-T7||7.5||-||-||-||-||No|| |
||
|- |
|- |
||
+ | |Pt||5 |
||
− | | Pt || 3 || 50(439V) || 0 || 20 || 45 || 0 || 0 || H2.75-T5 || 3.9 || - || - || - || - || Yes || Ning Cao |
||
+ | | ||200||0||20||45||0||0||H2.75-T5||7.4||-||-||-||-||Yes||Ning Cao |
||
+ | |- |
||
+ | |Pt||3 |
||
+ | | ||50(439V)||0||20||45||0||0||H2.75-T5||3.9||-||-||-||-||Yes||Ning Cao |
||
+ | |- |
||
+ | |Ru |
||
+ | |3 |
||
+ | | |
||
+ | |200 |
||
+ | | |
||
+ | | |
||
+ | |45 |
||
+ | | |
||
+ | | |
||
+ | |H2.75-T4 |
||
+ | |~10 |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | |Yes |
||
+ | |Ning Cao |
||
|- |
|- |
||
+ | |Ti||10 |
||
− | | Ti || 10 || 200 || 0 || 20 || 45 || 0 || 0 || H2.75-T5 || 2.3 || - || - || - || - || Yes || Ning Cao |
||
+ | | ||200||0||20||45||0||0||H2.75-T5||2.3||-||-||-||-||Yes||Ning Cao |
||
|- |
|- |
||
+ | |TiN||3 |
||
− | | TiN || 3 || 150 || 110V || 20 || 48.25 || 1.75 || 0 || H2.5-T5 || 2 || - || 60 || - || - || No || |
||
+ | | ||150||110V||20||48.25||1.75||0||H2.5-T5||2||-||60||-||-||No|| |
||
|- |
|- |
||
+ | |TiO<sub>2</sub>||3 |
||
− | | TiO<sub>2</sub> || 3 || 250(RF:450V) || 0 || 20 || 45 || 0 || 3 || H2.75-T5 ||4.3|| - || || - || - || Yes || Ning Cao |
||
+ | | ||250(RF:450V)||0||20||45||0||3||H2.75-T5||4.3||-|| ||-||-||Yes||Ning Cao |
||
|- |
|- |
||
+ | |TiW||4.5 |
||
− | | TiW || 4.5 || 200 || 0 || 20 || 45 || 0 || 0 || H1-T10 || 4.7 || - || - || - || - || Yes || Ning Cao |
||
+ | | ||200||0||20||45||0||0||H1-T10||4.7||-||-||-||-||Yes||Ning Cao |
||
|- |
|- |
||
+ | |TiW||4.5 |
||
− | | TiW || 4.5 || 300 || 0 || 75 || 45 || 0 || 0 || H2.75-T5 || 9.5 || -150 to 150 || 60 || - || - || Yes || 10%Ti by Wt |
||
+ | | ||300||0||75||45||0||0||H2.75-T5||9.5||-150 to 150||60||-||-||Yes||10%Ti by Wt |
||
|- |
|- |
||
+ | |W||3 |
||
− | | W || 3 || 300 || 0 || 50 || 45 || 0 || 0 || H2.75-T5 || 11.5 || -150 to 150 || 11 || - || - || Yes || Jeremy Watcher |
||
+ | | ||300||0||50||45||0||0||H2.75-T5||11.5||-150 to 150||11||-||-||Yes||Jeremy Watcher |
||
|- |
|- |
||
|} |
|} |
||
− | == W-TiW Deposition (Sputter 4) == |
||
− | *[[media:W-TiW-Sputtering-AJA-4-Data-Recipe-RevB.pdf|W-TiW Deposition Recipe]] |
||
− | == |
+ | ===Au Deposition (Sputter 4)=== |
− | *[[media:Ti-Au-Sputtering-Films-AJA2-rev1.pdf|Ti-Au Deposition Recipe and SEM Cross-Sections]] |
||
+ | *[//wiki.nanotech.ucsb.edu/wiki/images/0/01/Au-Sputter4-5mT-200W-120s.pdf Au Film's AFM Step and Roughness] |
||
− | == Pt Deposition (Sputter 4) == |
||
− | *[[media:Pt-Sputter4.pdf|Pt Film's AFM Step and Roughness]] |
||
− | == |
+ | ===Al Deposition (Sputter 4)=== |
− | *[[media:TiW-Sputter4-4.5mT-300W-300s.pdf|TiW Film's AFM Step and Roughness]] |
||
+ | *[//wiki.nanotech.ucsb.edu/wiki/images/1/17/Al-Sputter4-5mT-200W-30m.pdf Al Film SEM Profile] |
||
− | == TiO<sub>2</sub> Deposition (Sputter 4) == |
||
− | *[[media:TiO2 film using Sputter4.pdf|TiO<sub>2</sub> Film's Refractive Index Spectrum, Resistivity, AFM Roughness]] |
||
− | == |
+ | ===Al2O3 Deposition (Sputter 4)=== |
− | *[[media:Au-Sputter4-5mT-200W-120s.pdf|Au Film's AFM Step and Roughness]] |
||
+ | *Rate: 5.134 nm/min |
||
− | == Al Deposition (Sputter 4) == |
||
+ | *[https://en.wikipedia.org/wiki/Cauchy%27s_equation Cauchy] Refractive Index Params (fit from λ=190-1700nm, indicating transparency over this range) |
||
− | *[[media:Al-Sputter4-5mT-200W-30m.pdf|Al Film SEM Profile]] |
||
+ | **A = 1.626 |
||
+ | **B = 5.980E-3 |
||
+ | **C = 1.622E-4 |
||
− | == |
+ | ===Pt Deposition (Sputter 4)=== |
− | * Rate: 5.134 nm/min |
||
− | * [https://en.wikipedia.org/wiki/Cauchy%27s_equation Cauchy] Refractive Index Params (fit from λ=190-1700nm, indicating transparency over this range) |
||
− | ** A = 1.626 |
||
− | ** B = 5.980E-3 |
||
− | ** C = 1.622E-4 |
||
+ | *[//wiki.nanotech.ucsb.edu/wiki/images/a/ab/Pt-Sputter4.pdf Pt Film's AFM Step and Roughness] |
||
− | =[[Sputter 5 (Lesker AXXIS)]]= |
||
− | '''NOTE: The above title is incorrect, this tool is actually an AJA Sputter tool, similar to Sputter #3 and #4. Website updates pending.''' |
||
+ | === Ru Deposition (Sputter 4) === |
||
− | The recipes below are given as starting points from data obtained in the nanofab. For critical depositions, calibrations are recommended. |
||
+ | * [https://wiki.nanotech.ucsb.edu/w/images/f/f6/SiO2_Etch%2C_Ru_HardMask_-_Fluorine_ICP_Etch_Process_-_Ning_Cao_2019-06.pdf Ruthenium Hardmask for SiO2 Etching - Full Process Traveler] by Ning Cao |
||
+ | ** Deposition Rate ~10nm/min |
||
+ | ** See [[ICP Etching Recipes#SiO2 Etching|Fluorine-ICP > SiO2 Etching]] page for more info. |
||
+ | ===Ti-Au Deposition (Sputter 4)=== |
||
− | Please see [https://signupmonkey.ece.ucsb.edu/cgi-bin/users/browse.cgi?tool_ID=21 the] [https://signupmonkey.ece.ucsb.edu/cgi-bin/users/browse.cgi?tool_ID=60 SignupMonkey] page for a list of currently installed targets. |
||
+ | |||
+ | *[//wiki.nanotech.ucsb.edu/wiki/images/8/89/Ti-Au-Sputtering-Films-AJA2-rev1.pdf Ti-Au Deposition Recipe and SEM Cross-Sections] |
||
+ | |||
+ | ===TiO<sub>2</sub> Deposition (Sputter 4)=== |
||
+ | |||
+ | *[//wiki.nanotech.ucsb.edu/wiki/images/1/19/TiO2_film_using_Sputter4.pdf TiO<sub>2</sub> Film's Refractive Index Spectrum, Resistivity, AFM Roughness] |
||
+ | |||
+ | ===TiW Deposition (Sputter 4)=== |
||
+ | |||
+ | *[//wiki.nanotech.ucsb.edu/wiki/images/7/78/TiW-Sputter4-4.5mT-300W-300s.pdf TiW Film's AFM Step and Roughness] |
||
+ | ===W-TiW Deposition (Sputter 4)=== |
||
+ | |||
+ | *[//wiki.nanotech.ucsb.edu/wiki/images/c/cc/W-TiW-Sputtering-AJA-4-Data-Recipe-RevB.pdf W-TiW Deposition Recipe] |
||
+ | |||
+ | ==[[Sputter 5 (AJA ATC 2200-V)]]== |
||
+ | |||
+ | Please see the [https://signupmonkey.ece.ucsb.edu/cgi-bin/users/browse.cgi?tool_ID=60 SignupMonkey] page for a list of currently installed targets. |
||
+ | |||
+ | === Materials Table (Sputter 5) === |
||
+ | The recipes below are given as starting points from data obtained in the nanofab. For critical depositions, calibrations are recommended. |
||
{| class="wikitable sortable" |
{| class="wikitable sortable" |
||
|- |
|- |
||
− | ! |
+ | !Material!!P(mT) |
− | !Power Source!! |
+ | !Power Source!!Pow(W)!!Sub(V)!!T(C)!!Ar!!N2!!O2!!Height-Tilt!!Rate(nm/min)!!Stress(MPa)!!Rs(uOhm-cm)!!Rq(nm)!!n@633nm!!k@633nm!!LPDb/LPDa*!!Data Below!!Comment |
+ | |- |
||
+ | |Al |
||
+ | |5 |
||
+ | | |
||
+ | |250 |
||
+ | |0 |
||
+ | |20 |
||
+ | |45 |
||
+ | |0 |
||
+ | |0 |
||
+ | |H1-T10 |
||
+ | |2.5 |
||
+ | |22 |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | |No (SEM available) |
||
+ | |Ning |
||
|- |
|- |
||
|Al2O3 |
|Al2O3 |
||
Line 238: | Line 364: | ||
|Demis 2018-04-13 |
|Demis 2018-04-13 |
||
|- |
|- |
||
− | | |
+ | |SiO2||3 |
− | ||| |
+ | | ||250||120||20||45||0||2||H1.0-T10||2.32|| ||-||-||1.49||-||153/6384||No||Biljana |
|- |
|- |
||
− | | |
+ | |SiO2||3 |
− | ||| |
+ | | ||250||120||20||45||0||4.5||H1.0-T10||2.29||-515||-||0.210||1.49|| ||138/4445||No ( AFM available)||Biljana |
|- |
|- |
||
− | | |
+ | |SiO2||3 |
− | ||| |
+ | | ||250||120||20||45||0||6||H1.0-T10||2.32|| ||-||-||1.49||-||27/1515||Yes||Biljana |
|- |
|- |
||
|} |
|} |
||
+ | ''*LPD: light particle detection:'' |
||
+ | |||
+ | *''LPDb: light particle detection before deposition'' |
||
+ | *''LPDa: light particle detection after deposition'' |
||
+ | |||
+ | ===SiO2 Deposition (Sputter 5)=== |
||
− | *LPD-light particle detection |
||
− | *LPDb- light particle detection before deposition |
||
− | *LPDa- light particle detection after deposition |
||
− | == SiO2 Deposition (Sputter 5) == |
||
*[https://docs.google.com/spreadsheets/d/1kzrbXdUJNf_-FjLJd-PTrbGDhGCKNNxo_JaOXkSpAF8/edit#gid=Sputter#5 SiO2 film] |
*[https://docs.google.com/spreadsheets/d/1kzrbXdUJNf_-FjLJd-PTrbGDhGCKNNxo_JaOXkSpAF8/edit#gid=Sputter#5 SiO2 film] |
||
− | =[[Ion Beam Deposition (Veeco NEXUS)]]= |
+ | ==[[Ion Beam Deposition (Veeco NEXUS)]]== |
*[https://docs.google.com/spreadsheet/ccc?key=0AuBs1GfMrpnXcEdXanZQNko3X0lUcHhVUlNyYnVDUkE&usp=sharing IBD Calibrations Spreadsheet] - Records of historical film depositions (rates, indices), Uniformity etc. |
*[https://docs.google.com/spreadsheet/ccc?key=0AuBs1GfMrpnXcEdXanZQNko3X0lUcHhVUlNyYnVDUkE&usp=sharing IBD Calibrations Spreadsheet] - Records of historical film depositions (rates, indices), Uniformity etc. |
||
− | **'''All users are required to enter their calibration deps (simple test deps only)''' |
+ | **'''All users are required to enter their calibration deps (simple test deps only)''' |
*[https://docs.google.com/spreadsheets/d/1y704PRxvXf8bbqb79CrISnk2t0FeojYVJIjrAcBU2_w/edit#gid=sharing Particulates in SiO2 and Ta2O5 in 2015] |
*[https://docs.google.com/spreadsheets/d/1y704PRxvXf8bbqb79CrISnk2t0FeojYVJIjrAcBU2_w/edit#gid=sharing Particulates in SiO2 and Ta2O5 in 2015] |
||
− | ==SiO{{sub|2}} deposition (IBD)== |
+ | ===SiO{{sub|2}} deposition (IBD)=== |
+ | |||
− | *[[media: New IBD SiO2 Standard Recipe.pdf |SiO<sub>2</sub> Standard Recipe]] |
||
+ | ==== SiO<sub>2</sub> Historical Data ==== |
||
+ | *[//wiki.nanotech.ucsb.edu/wiki/images/8/8d/New_IBD_SiO2_Standard_Recipe.pdf SiO<sub>2</sub> Standard Recipe] |
||
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dFRJLUZUdXB4WFA1S1BMMWQ4WndpTWc&usp=drive_web#gid=sharing SiO<sub>2</sub> Data December 2014] |
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dFRJLUZUdXB4WFA1S1BMMWQ4WndpTWc&usp=drive_web#gid=sharing SiO<sub>2</sub> Data December 2014] |
||
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dGNyV083bmpzMjZpZ0JFVWhoOUpaN3c#gid=sharing SiO<sub>2</sub> Thickness uniformity 2014] |
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dGNyV083bmpzMjZpZ0JFVWhoOUpaN3c#gid=sharing SiO<sub>2</sub> Thickness uniformity 2014] |
||
Line 272: | Line 402: | ||
*[https://docs.google.com/spreadsheets/d/1dFI1B2WxS7oEGMPl2dlLtmiAin-6EKWSEj9hFezB4_w/edit#gid==sharing SiO<sub>2</sub> Thickness uniformity-1hr depositions 2016] |
*[https://docs.google.com/spreadsheets/d/1dFI1B2WxS7oEGMPl2dlLtmiAin-6EKWSEj9hFezB4_w/edit#gid==sharing SiO<sub>2</sub> Thickness uniformity-1hr depositions 2016] |
||
− | ==== |
+ | ====SiO<sub>2</sub> 1hr deposition properties:==== |
+ | |||
*Dep.rate: ≈ 5.2 nm/min (users must calibrate this prior to critical deps) |
*Dep.rate: ≈ 5.2 nm/min (users must calibrate this prior to critical deps) |
||
*HF e.r.~350 nm/min |
*HF e.r.~350 nm/min |
||
Line 278: | Line 409: | ||
*Refractive Index: ≈ 1.494 |
*Refractive Index: ≈ 1.494 |
||
*[[http://en.wikipedia.org/wiki/Cauchy's_equation Cauchy Parameters]] (350-2000nm): |
*[[http://en.wikipedia.org/wiki/Cauchy's_equation Cauchy Parameters]] (350-2000nm): |
||
− | ** |
+ | **A = 1.480 |
− | ** |
+ | **B = 0.00498 |
− | ** |
+ | **C = -3.2606e-5 |
+ | |||
− | ==Si<sub>3</sub>N<sub>4</sub> deposition (IBD)== |
||
− | + | ===Si<sub>3</sub>N<sub>4</sub> deposition (IBD)=== |
|
+ | |||
+ | *[//wiki.nanotech.ucsb.edu/wiki/images/d/d3/IBD_SiNdeposition.pdf Si<sub>3</sub>N<sub>4</sub> Standard Recipe] |
||
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dDE4RldRQnA1N1ptOUlHQVc3QjNXSkE#gid=sharing Si<sub>3</sub>N<sub>4</sub> Data December 2014] |
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dDE4RldRQnA1N1ptOUlHQVc3QjNXSkE#gid=sharing Si<sub>3</sub>N<sub>4</sub> Data December 2014] |
||
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dEdsbWRhYW9mbFRLem56TjFFWjRwR1E#gid=sharing Si<sub>3</sub>N<sub>4</sub> Thickness uniformity 2014] |
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dEdsbWRhYW9mbFRLem56TjFFWjRwR1E#gid=sharing Si<sub>3</sub>N<sub>4</sub> Thickness uniformity 2014] |
||
Line 291: | Line 424: | ||
*Refractive Index: ≈ 1.969 |
*Refractive Index: ≈ 1.969 |
||
*[[http://en.wikipedia.org/wiki/Cauchy's_equation Cauchy Parameters]] (350-2000nm): |
*[[http://en.wikipedia.org/wiki/Cauchy's_equation Cauchy Parameters]] (350-2000nm): |
||
− | ** |
+ | **A = 2.000 |
− | ** |
+ | **B = 0.01974 |
− | ** |
+ | **C = 1.2478e-4 |
− | == |
+ | ===SiO<sub>x</sub>N<sub>y</sub> deposition (IBD)=== |
These are some old (2010), initial characterizations only. A recipe improvement would be to increase the Assist O2+N2 = 60sccm total, increasing repeatability. Contact [[Demis D. John|Demis]] for more info. |
These are some old (2010), initial characterizations only. A recipe improvement would be to increase the Assist O2+N2 = 60sccm total, increasing repeatability. Contact [[Demis D. John|Demis]] for more info. |
||
{| |
{| |
||
Line 302: | Line 435: | ||
|} |
|} |
||
− | ==Ta{{sub|2}}O{{sub|5}} deposition (IBD)== |
+ | ===Ta{{sub|2}}O{{sub|5}} deposition (IBD)=== |
+ | ==== Ta2O5 Historical Data (IBD) ==== |
||
− | *[[media:IBD Ta2O5 deposition details.pdf|Ta{{sub|2}}O{{sub|5}} Standard Recipe]] |
||
+ | *[//wiki.nanotech.ucsb.edu/wiki/images/8/85/IBD_Ta2O5_deposition_details.pdf Ta{{sub|2}}O{{sub|5}} Standard Recipe] |
||
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dGhhUGdCR2JudkZJU3pBemR4bS1GWWc#gid=0=sharing Ta{{sub|2}}O{{sub|5}} Data December 2014] |
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dGhhUGdCR2JudkZJU3pBemR4bS1GWWc#gid=0=sharing Ta{{sub|2}}O{{sub|5}} Data December 2014] |
||
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dE5xbVFyUFZqdTdUN0JRSUNvMGFGb2c#gid=sharing Ta{{sub|2}}O{{sub|5}} Thickness uniformity 2014] |
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dE5xbVFyUFZqdTdUN0JRSUNvMGFGb2c#gid=sharing Ta{{sub|2}}O{{sub|5}} Thickness uniformity 2014] |
||
Line 315: | Line 449: | ||
*[https://docs.google.com/spreadsheets/d/1U7XUvluOpgD7tsciZ1pAFGiFsKJKvym6mH5hKaSt5b0/edit#gid=sharing Ta{{sub|2}}O{{sub|5}} Thickness uniformity-1hr depositions 2016] |
*[https://docs.google.com/spreadsheets/d/1U7XUvluOpgD7tsciZ1pAFGiFsKJKvym6mH5hKaSt5b0/edit#gid=sharing Ta{{sub|2}}O{{sub|5}} Thickness uniformity-1hr depositions 2016] |
||
+ | ==== Ta2O5 Deposition/Film Properies (IBD) ==== |
||
− | |||
*Ta2O5 1hr depositions: |
*Ta2O5 1hr depositions: |
||
*Deposition Rate: ≈ 7.8 nm/min (users must calibrate this prior to critical deps) |
*Deposition Rate: ≈ 7.8 nm/min (users must calibrate this prior to critical deps) |
||
Line 322: | Line 456: | ||
*Refractive Index: ≈ 2.172 |
*Refractive Index: ≈ 2.172 |
||
*[[http://en.wikipedia.org/wiki/Cauchy's_equation Cauchy Parameters]] (350-2000nm): |
*[[http://en.wikipedia.org/wiki/Cauchy's_equation Cauchy Parameters]] (350-2000nm): |
||
− | ** |
+ | **A = 2.1123 |
− | ** |
+ | **B = 0.018901 |
− | ** |
+ | **C = -0.016222 |
− | ==TiO{{sub|2}} deposition (IBD)== |
+ | ===TiO{{sub|2}} deposition (IBD)=== |
+ | |||
− | *[[media:New IBD TiO2 deposition.pdf|TiO<sub>2</sub> Standard Recipe]] |
||
+ | *[//wiki.nanotech.ucsb.edu/wiki/images/3/3b/New_IBD_TiO2_deposition.pdf TiO<sub>2</sub> Standard Recipe] |
||
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dGVXVkM4dEdXaU15M09HNGhJbGUycVE#gid=sharing TiO<sub>2</sub> Data December 2014] |
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dGVXVkM4dEdXaU15M09HNGhJbGUycVE#gid=sharing TiO<sub>2</sub> Data December 2014] |
||
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dF9YSW9jTDJzY19MbmVEbUQtVzJVdVE#gid=sharing TiO<sub>2</sub> Thickness uniformity 2014] |
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dF9YSW9jTDJzY19MbmVEbUQtVzJVdVE#gid=sharing TiO<sub>2</sub> Thickness uniformity 2014] |
||
Line 336: | Line 471: | ||
*Refractive Index: ≈ 2.259 |
*Refractive Index: ≈ 2.259 |
||
*[[http://en.wikipedia.org/wiki/Cauchy's_equation Cauchy Parameters]] (350-2000nm): |
*[[http://en.wikipedia.org/wiki/Cauchy's_equation Cauchy Parameters]] (350-2000nm): |
||
− | ** |
+ | **A = 2.435 |
− | ** |
+ | **B = -4.9045e-4 |
− | ** |
+ | **C = 0.01309 |
*Absorbing < ~350nm |
*Absorbing < ~350nm |
||
− | == |
+ | ===Al<sub>2</sub>O<sub>3</sub> deposition (IBD)=== |
− | * Al2O3 standard recipe ( working on) |
||
+ | *Al2O3 standard recipe: 1_Al2O3_dep |
||
− | * [https://docs.google.com/spreadsheets/d/1Qwxa7rtq2kGeFUQxnjGFgtdCJP4uIX_bdUcCWFvO72g/edit#gid= Al2O3 Data 2018] |
||
+ | |||
− | * [https://docs.google.com/spreadsheets/d/1rjwDQ0WJOIL7XWx2KWQ4fEPjNkr6GEmiXGmQXZnWFOI/edit#gid= Al2O3 Thickness uniformity 2018] |
||
+ | *[https://docs.google.com/spreadsheets/d/1Qwxa7rtq2kGeFUQxnjGFgtdCJP4uIX_bdUcCWFvO72g/edit#gid= Al2O3 Data 2018] |
||
+ | *[https://docs.google.com/spreadsheets/d/1rjwDQ0WJOIL7XWx2KWQ4fEPjNkr6GEmiXGmQXZnWFOI/edit#gid= Al2O3 Thickness uniformity 2018] |
||
*Deposition Rate: ≈ 2.05nm/min (users must calibrate this prior to critical deps) |
*Deposition Rate: ≈ 2.05nm/min (users must calibrate this prior to critical deps) |
||
Line 352: | Line 488: | ||
*Refractive Index: ≈ 1.656 |
*Refractive Index: ≈ 1.656 |
||
*[[http://en.wikipedia.org/wiki/Cauchy's_equation Cauchy Parameters]] (350-2000nm):( working on) |
*[[http://en.wikipedia.org/wiki/Cauchy's_equation Cauchy Parameters]] (350-2000nm):( working on) |
||
− | ** |
+ | **A = |
− | ** |
+ | **B = |
− | ** |
+ | **C = |
*Absorbing < ~350nm |
*Absorbing < ~350nm |
||
+ | |||
+ | == Reference Recipes (Disabled Tools) == |
||
+ | |||
+ | === [[Sputter 2 (SFI Endeavor)|<big><u>Sputter 2 (SFI Endeavor)</u></big>]] === |
||
+ | '''This Tool has been Disabled, and is not available for use any more! These recipes are displayed here for historical/reference purposes only.''' |
||
+ | '''Al Deposition (Sputter 2)''' |
||
+ | *[//wiki.nanotech.ucsb.edu/wiki/images/0/05/20-Al-Sputtering-Film-Sputter-2.pdf Al Deposition Recipe] |
||
+ | '''AlN<sub>x</sub> Deposition (Sputter 2)''' |
||
+ | *[//wiki.nanotech.ucsb.edu/wiki/images/8/8c/Sputter-2-AlN-Endeavor-rev1.pdf AlN<sub>x</sub> Deposition Recipe] |
||
+ | '''Au Deposition (Sputter 2)''' |
||
+ | *[//wiki.nanotech.ucsb.edu/wiki/images/8/8a/21-Au-Sputter-film-recipes-Sputter-2.pdf Au Deposition Recipe] |
||
+ | '''TiO<sub>2</sub> Deposition (Sputter 2)''' |
||
+ | *[//wiki.nanotech.ucsb.edu/wiki/images/c/c4/22-TiO2-Film-Sputter-2.pdf TiO2<sub>2</sub> Deposition Recipe] |
Revision as of 18:32, 16 April 2021
Back to Vacuum Deposition Recipes. R
Sputter 3 (AJA ATC 2000-F)
Please see the SignupMonkey Page for a list of currently installed targets.
Materials Table (Sputter 3)
The recipes below are given as starting points from data obtained in the nanofab. For critical depositions, calibrations are recommended.
Material | P(mT) | Pow(W) | Sub(W) | T(C) | Ar | N2 | O2 | Height-Tilt | Rate(nm/min) | Stress(MPa) | Rs(uOhm-cm) | n@633nm | k@633nm | Target Consumed Lower Limit | Data Below | Comment |
---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
Au | - | - | - | - | - | - | - | - | - | - | - | - | - | Set: 200 W
Read: 400 VDC |
no | |
Al2O3 | 3 | 200 (RF2) | off | 20 | 30 | 1.5 | 1.52"-4mm | 5.32 | 1.6478 | 0 | no | Demis D. John | ||||
Co | 10(5) | 200 | 0 | 20 | 25 | 0 | 0 | 25-9 | 2.3 | - | - | - | - | yes | Alex K | |
Cr | 5 | 200 | 0 | 20 | 25 | 0 | 0 | 44-4 | 6.84 | - | - | - | - | no | Brian | |
Cu | 1.5 | 50(395v) | 0 | 20 | 25 | 0 | 0 | 25-9 | 4.15 | - | - | - | - | no | Ning | |
Cu | 5 | 150(~490v) | 0 | 20 | 15 | 0 | 0 | 0.82"-9 | 8 | - | - | - | - | yes | Ning | |
Fe | 10(5) | 200 | 0 | 20 | 25 | 0 | 0 | 25-9 | 1.25 | - | - | - | - | No | Alex K | |
Mo | 3 | 200 | 0 | 20 | 25 | 0 | 0 | 44-4 | 13.15 | - | - | - | - | yes | Ning | |
Ni | 5 | 150 | 0 | 20 | 25 | 0 | 0 | 44-4 | 5.23 | - | - | - | - | yes | Ning | |
Ni | 5 | 150 | 0 | 20 | 25 | 0 | 0 | 25-9 | 1.82 | - | - | - | - | yes | Ning | |
Ni | 5 | 75 | 0 | 20 | 25 | 0 | 0 | 44-4 | 2.50 | - | - | - | - | yes | Ning | |
Ni | 3 | 200 | 0 | 20 | 25 | 0 | 0 | 44-4 | 9.4 | - | - | - | - | yes | Ning | |
Ni | 1.5 | 50(399v) | 0 | 20 | 25 | 0 | 0 | 25-9 | 0.96 | - | - | - | - | no | Ning | |
Pt | 3 | 50 | 0 | 20 | 25 | 0 | 0 | 0.82"-9 | 2.9 | - | - | - | - | no | Ning | |
Si | 8 | 250 | 0 | 25 | 25 | 0 | 0 | 15-3 | 1.4 | - | - | - | - | no | Gerhard - ramp 2W/s - 3% Unif 4" wafer | |
SiN | 3 | 200 | 10 | 20 | 25 | 3 | 0 | 25-9 | 1.56 | - | - | 1.992 | - | yes | Brian | |
SiN | 3 | 250 | 10 | 20 | 25 | 2.5 | 0 | 25-9 | 2.1 | - | - | 2.06 | - | yes | Brian | |
SiO2 | 3 | 200 | 10 | 20 | 25 | 0 | 3 | 25-9 | 3.68 | - | - | 1.447 | - | yes | Brian | |
SiO2 | 3 | 200 | 10 | 20 | 25 | 0 | 5 | 45-3 | 2.60 | - | - | 1.471 | - | yes | Brian | |
SiO2 | 3 | 250 | 10 | 20 | 25 | 0 | 2.5 | 25-9 | 4.3 | - | - | 1.485 | - | yes | Brian | |
Ta | 5 | 150 | 0 | 20 | 25 | 0 | 0 | 44-4 | 9.47 | - | - | - | - | yes | Ning | |
Ta | 5 | 75 | 0 | 20 | 25 | 0 | 0 | 44-4 | 5.03 | - | - | - | - | yes | Ning | |
Ti | 3 | 100 | 0 | 20 | 25 | 0 | 0 | 25-9 | 1.34 | - | - | - | - | yes | Ning | |
SampleClean-NativeSiO2 | 10 | 0 | 18 | 20 | 25 | 0 | 0 | 44-4 | - | - | - | - | - | yes | 150Volts 5 min |
Height Conversion for Older Recipes
Old recipes using the manual Height setting in millimeters can be converted to the new programmatic settings in inches as follows:
Old (mm) | New (inches) | Typical Gun Tilt (mm) |
---|---|---|
15 | ||
25 | 0.82 | 9 |
44 | 1.52 | 4 |
Interpolation plot can be found here.
Fe and Co Deposition (Sputter 3)
Cu Deposition (Sputter 3)
Mo Deposition (Sputter 3)
Ni and Ta Deposition (Sputter 3)
SiO2 Deposition (Sputter 3)
SiN Deposition (Sputter 3)
Ti Deposition (Sputter 3)
Sputter 4 (AJA ATC 2200-V)
Please see the SignupMonkey page for a list of currently installed targets.
Materials Table (Sputter 4)
The recipes below are given as starting points from data obtained in the nanofab. For critical depositions, calibrations are recommended.
Material | P(mT) | Power Source | Pow(W) | Sub(W) | T(C) | Ar | N2 | O2 | Height-Tilt | Rate(nm/min) | Stress(MPa) | Rs(uOhm-cm) | n@633nm | k@633nm | Data Below | Comment |
---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
Al | 5 | 200 | 0 | 20 | 45 | 0 | 0 | H2.75-T5 | 4.4 | - | - | - | - | Yes | Ning Cao | |
Al2O3 | 3 | RF4-Sw1 | 200 | 0 | 20 | 30 | 0 | 1.5 | H2.75-T5 | 5.1 | 1.64202 | 0 | partial | Demis D. John | ||
Au | 5 | 200 | 0 | 20 | 45 | 0 | 0 | H1-T10 | 17.7 | - | - | - | - | Yes | Ning Cao | |
Au | 10 | 300 | 0 | 20 | 45 | 0 | 0 | H2.75-T5 | 45.4 | - | - | - | - | Yes | Ning Cao | |
Cu | 5 | 150 | 0 | 20 | 30 | 0 | 0 | H0.82-T9 | 6.7 | No (SEM available) | Ning Cao | |||||
Nb | 4 | 250 | 0 | 20 | 30 | 0 | 0 | H2.00-T7 | 7.5 | - | - | - | - | No | ||
Pt | 5 | 200 | 0 | 20 | 45 | 0 | 0 | H2.75-T5 | 7.4 | - | - | - | - | Yes | Ning Cao | |
Pt | 3 | 50(439V) | 0 | 20 | 45 | 0 | 0 | H2.75-T5 | 3.9 | - | - | - | - | Yes | Ning Cao | |
Ru | 3 | 200 | 45 | H2.75-T4 | ~10 | Yes | Ning Cao | |||||||||
Ti | 10 | 200 | 0 | 20 | 45 | 0 | 0 | H2.75-T5 | 2.3 | - | - | - | - | Yes | Ning Cao | |
TiN | 3 | 150 | 110V | 20 | 48.25 | 1.75 | 0 | H2.5-T5 | 2 | - | 60 | - | - | No | ||
TiO2 | 3 | 250(RF:450V) | 0 | 20 | 45 | 0 | 3 | H2.75-T5 | 4.3 | - | - | - | Yes | Ning Cao | ||
TiW | 4.5 | 200 | 0 | 20 | 45 | 0 | 0 | H1-T10 | 4.7 | - | - | - | - | Yes | Ning Cao | |
TiW | 4.5 | 300 | 0 | 75 | 45 | 0 | 0 | H2.75-T5 | 9.5 | -150 to 150 | 60 | - | - | Yes | 10%Ti by Wt | |
W | 3 | 300 | 0 | 50 | 45 | 0 | 0 | H2.75-T5 | 11.5 | -150 to 150 | 11 | - | - | Yes | Jeremy Watcher |
Au Deposition (Sputter 4)
Al Deposition (Sputter 4)
Al2O3 Deposition (Sputter 4)
- Rate: 5.134 nm/min
- Cauchy Refractive Index Params (fit from λ=190-1700nm, indicating transparency over this range)
- A = 1.626
- B = 5.980E-3
- C = 1.622E-4
Pt Deposition (Sputter 4)
Ru Deposition (Sputter 4)
- Ruthenium Hardmask for SiO2 Etching - Full Process Traveler by Ning Cao
- Deposition Rate ~10nm/min
- See Fluorine-ICP > SiO2 Etching page for more info.
Ti-Au Deposition (Sputter 4)
TiO2 Deposition (Sputter 4)
TiW Deposition (Sputter 4)
W-TiW Deposition (Sputter 4)
Sputter 5 (AJA ATC 2200-V)
Please see the SignupMonkey page for a list of currently installed targets.
Materials Table (Sputter 5)
The recipes below are given as starting points from data obtained in the nanofab. For critical depositions, calibrations are recommended.
Material | P(mT) | Power Source | Pow(W) | Sub(V) | T(C) | Ar | N2 | O2 | Height-Tilt | Rate(nm/min) | Stress(MPa) | Rs(uOhm-cm) | Rq(nm) | n@633nm | k@633nm | LPDb/LPDa* | Data Below | Comment |
---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
Al | 5 | 250 | 0 | 20 | 45 | 0 | 0 | H1-T10 | 2.5 | 22 | No (SEM available) | Ning | ||||||
Al2O3 | 1.5 | DC5-SW1 | 150 | - | - | 45 | - | 5 | H2.75-T5 | 5.3 | ? | ? | ? | 1.641 | - | ? | No | Demis 2018-04-13 |
SiO2 | 3 | 250 | 120 | 20 | 45 | 0 | 2 | H1.0-T10 | 2.32 | - | - | 1.49 | - | 153/6384 | No | Biljana | ||
SiO2 | 3 | 250 | 120 | 20 | 45 | 0 | 4.5 | H1.0-T10 | 2.29 | -515 | - | 0.210 | 1.49 | 138/4445 | No ( AFM available) | Biljana | ||
SiO2 | 3 | 250 | 120 | 20 | 45 | 0 | 6 | H1.0-T10 | 2.32 | - | - | 1.49 | - | 27/1515 | Yes | Biljana |
*LPD: light particle detection:
- LPDb: light particle detection before deposition
- LPDa: light particle detection after deposition
SiO2 Deposition (Sputter 5)
Ion Beam Deposition (Veeco NEXUS)
- IBD Calibrations Spreadsheet - Records of historical film depositions (rates, indices), Uniformity etc.
- All users are required to enter their calibration deps (simple test deps only)
- Particulates in SiO2 and Ta2O5 in 2015
SiO2 deposition (IBD)
SiO2 Historical Data
- SiO2 Standard Recipe
- SiO2 Data December 2014
- SiO2 Thickness uniformity 2014
- SiO2 Data-15min depositions 2015
- SiO2 Thickness uniformity-15 min depositions 2015
- SiO2 Data-1hr depositions 2015
- SiO2 Thickness uniformity-1hr depositions 2015
- SiO2 Data-1hr depositions 2016
- SiO2 Thickness uniformity-1hr depositions 2016
SiO2 1hr deposition properties:
- Dep.rate: ≈ 5.2 nm/min (users must calibrate this prior to critical deps)
- HF e.r.~350 nm/min
- Stress ≈ -390MPa (compressive)
- Refractive Index: ≈ 1.494
- [Cauchy Parameters] (350-2000nm):
- A = 1.480
- B = 0.00498
- C = -3.2606e-5
Si3N4 deposition (IBD)
- Deposition Rate: ≈ 4.10 nm/min (users must calibrate this prior to critical deps)
- HF e.r.~11nm/min
- Stress ≈ -1590MPa (compressive)
- Refractive Index: ≈ 1.969
- [Cauchy Parameters] (350-2000nm):
- A = 2.000
- B = 0.01974
- C = 1.2478e-4
SiOxNy deposition (IBD)
These are some old (2010), initial characterizations only. A recipe improvement would be to increase the Assist O2+N2 = 60sccm total, increasing repeatability. Contact Demis for more info.
Ta2O5 deposition (IBD)
Ta2O5 Historical Data (IBD)
- Ta2O5 Data December-15 min depositions 2015
- Ta2O5 Thickness uniformity-15 min depositions 2015
- Ta2O5 Data December-1hr depositions 2015
- Ta2O5 Thickness uniformity-1hr depositions 2015
- Ta2O5 Data December-1hr depositions 2016
- Ta2O5 Thickness uniformity-1hr depositions 2016
Ta2O5 Deposition/Film Properies (IBD)
- Ta2O5 1hr depositions:
- Deposition Rate: ≈ 7.8 nm/min (users must calibrate this prior to critical deps)
- HF e.r.~2 nm/min
- Stress ≈ -232MPa (compressive)
- Refractive Index: ≈ 2.172
- [Cauchy Parameters] (350-2000nm):
- A = 2.1123
- B = 0.018901
- C = -0.016222
TiO2 deposition (IBD)
- Deposition Rate: ≈ 1.29 nm/min (users must calibrate this prior to critical deps)
- HF etch rate ~5.34nm/min
- Stress ≈ -445MPa (compressive)
- Refractive Index: ≈ 2.259
- [Cauchy Parameters] (350-2000nm):
- A = 2.435
- B = -4.9045e-4
- C = 0.01309
- Absorbing < ~350nm
Al2O3 deposition (IBD)
- Al2O3 standard recipe: 1_Al2O3_dep
- Deposition Rate: ≈ 2.05nm/min (users must calibrate this prior to critical deps)
- HF etch rate ~167nm/min
- Stress ≈ -332MPa (compressive)
- Refractive Index: ≈ 1.656
- [Cauchy Parameters] (350-2000nm):( working on)
- A =
- B =
- C =
- Absorbing < ~350nm
Reference Recipes (Disabled Tools)
Sputter 2 (SFI Endeavor)
This Tool has been Disabled, and is not available for use any more! These recipes are displayed here for historical/reference purposes only.
Al Deposition (Sputter 2)
AlNx Deposition (Sputter 2)
Au Deposition (Sputter 2)
TiO2 Deposition (Sputter 2)