Line 330: | Line 330: | ||
*{{fl|UV6-Positive-Resist-Datasheet.pdf|UV6-0.8}} | *{{fl|UV6-Positive-Resist-Datasheet.pdf|UV6-0.8}} | ||
*{{fl|UV26-Positive-Resist-Datasheet.pdf|UV26-2.5}} | *{{fl|UV26-Positive-Resist-Datasheet.pdf|UV26-2.5}} | ||
− | |||
;<div id="NegativePR"><big>Negative Photoresists</big></div> | ;<div id="NegativePR"><big>Negative Photoresists</big></div> | ||
Line 348: | Line 347: | ||
*{{fl|UVN-30_-_Negative-Resist-Datasheet_-_Apr_2004.pdf|UVN-30-0.8}} | *{{fl|UVN-30_-_Negative-Resist-Datasheet_-_Apr_2004.pdf|UVN-30-0.8}} | ||
− | |||
;<div id="Underlayers"><big>Underlayers</big></div> | ;<div id="Underlayers"><big>Underlayers</big></div> | ||
Line 354: | Line 352: | ||
*{{fl|PMGI-Underlayer-Datasheet.pdf|PMGI (PMGI SF3,5,8,11,15)}} | *{{fl|PMGI-Underlayer-Datasheet.pdf|PMGI (PMGI SF3,5,8,11,15)}} | ||
*{{fl|LOL2000-Underlayer-Datasheet.pdf|Shipley LOL2000}} | *{{fl|LOL2000-Underlayer-Datasheet.pdf|Shipley LOL2000}} | ||
− | |||
;<div id="EBLPR"><big>E-beam resists</big></div> | ;<div id="EBLPR"><big>E-beam resists</big></div> | ||
Line 360: | Line 357: | ||
*{{fl|PMMA-E-Beam-Resist-Datasheet.pdf|PMMA (PMMA, P(MMA-MAA) copolymer)}} | *{{fl|PMMA-E-Beam-Resist-Datasheet.pdf|PMMA (PMMA, P(MMA-MAA) copolymer)}} | ||
*{{fl|maN2403-E-Beam-Resist-Datasheet.pdf|maN 2403}} | *{{fl|maN2403-E-Beam-Resist-Datasheet.pdf|maN 2403}} | ||
− | |||
;<div id="NanoImprinting"><big>Nanoimprinting</big></div> | ;<div id="NanoImprinting"><big>Nanoimprinting</big></div> | ||
Line 373: | Line 369: | ||
*{{fl|CEM365iS-Contrast-Enhancement-Datasheet.pdf|CEM365iS}} | *{{fl|CEM365iS-Contrast-Enhancement-Datasheet.pdf|CEM365iS}} | ||
− | |||
;<div id="AntiReflectionCoatings"><big>Anti-Reflection Coatings</big></div> | ;<div id="AntiReflectionCoatings"><big>Anti-Reflection Coatings</big></div> | ||
Line 380: | Line 375: | ||
*{{fl|DUV42P-Anti-Reflective-Coating.pdf|DUV42P (DUV) (For AR2 replacement)}} | *{{fl|DUV42P-Anti-Reflective-Coating.pdf|DUV42P (DUV) (For AR2 replacement)}} | ||
*{{fl|DS-K101-304-Anti-Reflective-Coating.pdf|DS-K101-304 (DUV developable BARC)}} | *{{fl|DS-K101-304-Anti-Reflective-Coating.pdf|DS-K101-304 (DUV developable BARC)}} | ||
− | |||
;<div id="AdhesionPromoters"><big>Adhesion Promoters</big></div> | ;<div id="AdhesionPromoters"><big>Adhesion Promoters</big></div> | ||
Line 388: | Line 382: | ||
*{{fl|OMNICOAT-revA.pdf|Omnicoat, SU-8 Adhesion Promoter}} | *{{fl|OMNICOAT-revA.pdf|Omnicoat, SU-8 Adhesion Promoter}} | ||
*{{fl|OrmoPrime-NIL-Adhesion-RevA.pdf|Ormoprime08-Ormostsmp Adhesion Promoter}} | *{{fl|OrmoPrime-NIL-Adhesion-RevA.pdf|Ormoprime08-Ormostsmp Adhesion Promoter}} | ||
− | |||
;<div id="SpinOnDielectrics"><big>Spin-On Dielectrics</big></div> | ;<div id="SpinOnDielectrics"><big>Spin-On Dielectrics</big></div> | ||
Line 400: | Line 393: | ||
*{{fl|512B-Datasheet-revA.pdf|Spin-on-Glass, Honeywell 512B (Not Photosensitive)}} | *{{fl|512B-Datasheet-revA.pdf|Spin-on-Glass, Honeywell 512B (Not Photosensitive)}} | ||
*{{fl|512B-Application-Data-Bake-revA.pdf|Honeywell 512B Apps Data}} | *{{fl|512B-Application-Data-Bake-revA.pdf|Honeywell 512B Apps Data}} | ||
− | |||
;<div id="Developers"><big>Developers</big></div> | ;<div id="Developers"><big>Developers</big></div> | ||
Line 409: | Line 401: | ||
*SU-8 Developer | *SU-8 Developer | ||
*101A Developer (for DUV Flood Exposed PMGI) | *101A Developer (for DUV Flood Exposed PMGI) | ||
− | |||
;<div id="PRRemovers"><big>Photoresist Removers</big></div> | ;<div id="PRRemovers"><big>Photoresist Removers</big></div> |
Revision as of 14:06, 17 June 2020
General Information
This page contains information and links to recipes/datasheets spin-coated materials used in the facility.
Table of Contents |
---|
|
Photolithography Recipes
- R = Recipe is available. Clicking this link will take you to the recipe.
- A = Material is available for use, but no recipes are provided.
Photolithography Recipes
| ||||||||
---|---|---|---|---|---|---|---|---|
Contact Aligner Recipes | Steppers Recipes | |||||||
Positive Resists | SUSS MJB-3 | SUSS MA-6 | Stepper 1 (GCA 6300) |
Stepper 2 (AutoStep 200) |
Stepper 3 (ASML DUV) |
MLA150 (Heidelberg) | ||
AZ4110 | R | R | A | A | ||||
AZ4210 | R | R | A | A | ||||
AZ4330RS | R | R | A | A | ||||
OCG 825-35CS | A | A | A | A | ||||
SPR 950-0.8 | A | A | A | A | ||||
SPR 955 CM-0.9 | A | R | R | R | ||||
SPR 955 CM-1.8 | A | A | R | R | ||||
SPR 220-3.0 | R | R | R | R | ||||
SPR 220-7.0 | R | R | R | R | ||||
THMR-IP3600 HP D | A | A | ||||||
UV6-0.8 | R | |||||||
UV210-0.3 | R | |||||||
UV26-2.5 | A | |||||||
Negative Resists | SUSS MJB-3 | SUSS MA-6 | Stepper 1 (GCA 6300) |
Stepper 2 (AutoStep 200) |
Stepper 3 (ASML DUV) |
MLA150 (Heidelberg) | ||
AZ5214-EIR | R | R | R | R | ||||
AZnLOF 2020 | R | R | R | R | ||||
AZnLOF 2035 | A | A | A | A | ||||
AZnLOF 2070 | A | A | A | A | ||||
AZnLOF 5510 | A | A | R | R | ||||
UVN30-0.8 | R | |||||||
SU-8 2005,2010, 2015 | A | R | A | A | ||||
SU-8 2075 | A | A | A | A | ||||
NR9-1000,3000,6000PY | R | R | A | R | ||||
Anti-Reflection Coatings | SUSS MJB-3 | SUSS MA-6 | Stepper 1 (GCA 6300) |
Stepper 2 (AutoStep 200) |
Stepper 3 (ASML DUV) |
MLA150 (Heidelberg) | ||
DUV42-P | R | |||||||
DS-K101-304 | R | |||||||
SUSS MJB-3 | SUSS MA-6 | Stepper 1 (GCA 6300) |
Stepper 2 (AutoStep 200) |
Stepper 3 (ASML DUV) |
MLA150 (Heidelberg) |
E-Beam Lithography Recipes
- Under Development.
Automated Coat/Develop System Recipes (S-Cubed Flexi)
Recipes pre-loaded on the S-Cubed Flexi automated coat/bake/develop system. Only staff may write new recipes, contact the tool supervisor for more info.
To Be Added
Nanoimprinting Recipes
- Thermal Nanoimprint Process and Tutorial
- UV-Cure Low Temp, Low Pressure, Soft-Stamp Nanoimprint Process
Holography Recipes
- Standard Holography Process - on SiO2 on Si
- Holography Process Variations - Set-up Angle - Etching into SiO2 and Si
- Etch SiO2 Nano-structure - Changing Side-wall Angle - Etching into Si with a different line-width
- Reduce SiO2 Nanowire Diameter - Thermal Oxidation - Vapor HF Etching
Low-K Spin-On Dielectric Recipes
Lift-Off Techniques
- Lift-Off Description/Tutorial
- How it works, process limits and considerations for designing your process
- I-Line Lift-Off: Bi-Layer Process with PMGI Underlayer and Contact Aligner
- DUV Lift-Off: UV6 Imaging Resist + PMGI Underlayer
Chemicals Stocked + Datasheets
The following is a list of the lithography chemicals we stock in the lab, with links to the datasheets for each. The datasheets will often have important processing info such as spin-speed vs. thickness curves, typical process parameters, bake temps/times etc.