The wafers used for process calibration are ordered from SVM. These are 4 inch silicon wafers with low particle count (LPD= light particle detection<100). The box with 25 wafers is stored in the cleanroom and used only for process calibration. Wafers are handled very carefully, because with every loading and unloading some particles will be added. |
The wafers used for process calibration are ordered from SVM. These are 4 inch silicon wafers with low particle count (LPD= light particle detection<100). The box with 25 wafers is stored in the cleanroom and used only for process calibration. Wafers are handled very carefully, because with every loading and unloading some particles will be added. |
||
− | == |
+ | == Scanning procedure == |
− | |||
+ | === before process calibration === |
||
# Log in (access code is boss) |
# Log in (access code is boss) |
||
# Load desired number of Si wafers to the carrier that says " SURFSCAN" . |
# Load desired number of Si wafers to the carrier that says " SURFSCAN" . |
||
Line 21: | Line 21: | ||
# Wafers are ready for process calibration |
# Wafers are ready for process calibration |
||
− | === |
+ | === after process calibration === |
# Log in (access code is boss) |
# Log in (access code is boss) |
||
Line 39: | Line 39: | ||
# Select "Home" so indexer moves up to loading/unloading positon |
# Select "Home" so indexer moves up to loading/unloading positon |
||
# Unload the wafers |
# Unload the wafers |
||
+ | |||
+ | == Plotting data == |
Revision as of 16:18, 31 March 2020
The wafers used for process calibration are ordered from SVM. These are 4 inch silicon wafers with low particle count (LPD= light particle detection<100). The box with 25 wafers is stored in the cleanroom and used only for process calibration. Wafers are handled very carefully, because with every loading and unloading some particles will be added.
Scanning procedure
before process calibration
- Log in (access code is boss)
- Load desired number of Si wafers to the carrier that says " SURFSCAN" .
- Place the carrier with wafers to the right indexer.
- Select in the menu option "CAS" (this will read all wafers that are in the carrier)
- Load one of standard recipes
- Select one of the recipes:
- UCSB Gain4 ( measuring small particles 0.16-2.8um)
- UCSB Gain2 ( measuring larger particles 2.8-28um)
- Select one of the recipe, modify it if needed, default the bin
- Select the wafer you want to scan
- Press SCAN
- Wait until scan is finished
- Record: LPD, particles #1, particles #8, haze
- Take a picture of the scan (by phone)
- Select "Home" so indexer moves up to loading/unloading positon
- Wafers are ready for process calibration
after process calibration
- Log in (access code is boss)
- Load treated Si wafers to the carrier that says " SURFSCAN" .
- Place the carrier with wafers to the right indexer.
- Select in the menu option "CAS" (this will read all wafers that are in the carrier)
- Load one of standard recipes
- Select one of the recipes :
- UCSB Gain4 ( measuring small particles 0.16-2.8um)
- UCSB Gain2 ( measuring larger particles 2.8-28um)
- Select one of the recipe, modify it if needed, default the bin
- Select the wafer you want to scan
- Press SCAN
- Wait until scan is finished
- Record: LPD, particles #1, particles #8, haze
- Take a picture of the scan (by phone)
- Select "Home" so indexer moves up to loading/unloading positon
- Unload the wafers