Difference between revisions of "Test Data of etching SiO2 with CHF3/CF4/O2 (using this recipe only for Fluorine etch of the underneath layer)"
Jump to navigation
Jump to search
(moved SEM images to table, changed "File:" link --> Direct link to file) |
|||
Line 1: | Line 1: | ||
{| class="wikitable" |
{| class="wikitable" |
||
| colspan="5" |ICP#2: 0.5Pa, 50/500W, CHF3/CF4/O2=35/5/10sccm, time=210 sec |
| colspan="5" |ICP#2: 0.5Pa, 50/500W, CHF3/CF4/O2=35/5/10sccm, time=210 sec |
||
+ | | |
||
|- |
|- |
||
|Date |
|Date |
||
Line 7: | Line 8: | ||
|Etch Selectivity (SiO2/PR) |
|Etch Selectivity (SiO2/PR) |
||
|Averaged Sidewall Angle (<sup>o</sup>) |
|Averaged Sidewall Angle (<sup>o</sup>) |
||
+ | |SEM Images |
||
|- |
|- |
||
|10/5/2018 |
|10/5/2018 |
||
Line 13: | Line 15: | ||
|0.74 |
|0.74 |
||
|77.9 |
|77.9 |
||
+ | | |
||
|- |
|- |
||
|1/28/2019 |
|1/28/2019 |
||
Line 19: | Line 22: | ||
|0.77 |
|0.77 |
||
| |
| |
||
⚫ | |||
|} |
|} |
||
⚫ |
Revision as of 00:03, 30 January 2019
ICP#2: 0.5Pa, 50/500W, CHF3/CF4/O2=35/5/10sccm, time=210 sec | |||||
Date | Sample# | Etch Rate (nm/min) | Etch Selectivity (SiO2/PR) | Averaged Sidewall Angle (o) | SEM Images |
10/5/2018 | SiO2#01 | 95.2 | 0.74 | 77.9 | |
1/28/2019 | I21902 | 92.1 | 0.77 | [1] |