ICP#2: 0.5Pa, 50/900W, CHF3/CF4=10/30 sccm, time=210 sec | ||||
Date | Sample# | Etch Rate (nm/min) | Etch Selectivity (SiO2/PR) | Averaged Sidewall Angle (o) |
10/5/2018 | SiO2#02 | 160 | 1.2 | 82.1 |