Difference between revisions of "Packaging Recipes"
(11 intermediate revisions by 2 users not shown) | |||
Line 2: | Line 2: | ||
== [[Dicing Saw (ADT)|Dicing Saw Recipes (ADT 7100)]] == |
== [[Dicing Saw (ADT)|Dicing Saw Recipes (ADT 7100)]] == |
||
− | === |
+ | === Recommended Dicing Parameters === |
+ | This table is for our stocked Resnoid blades: -4C blades are 4mils/100µm wide, while -8C blades are 8mils/200µm wide. Plan for ~50–100µm extra edge clearance to account for chipping etc. |
||
⚫ | |||
+ | |||
− | | colspan="4" |Recommended Dicing Parameters |
||
+ | Narrower (~30-50µm) Nickel Hubbed blades are often used for even narrower dicing streets, these must be purchased by the user. |
||
⚫ | |||
+ | {| class="wikitable sortable" |
||
⚫ | |||
⚫ | |||
⚫ | |||
⚫ | |||
|- |
|- |
||
− | + | !Material |
|
− | + | !Blade P/N |
|
− | + | !Spindle Speed |
|
+ | (KRPM) |
||
− | + | !Cut Speed |
|
+ | (mm/s) |
||
|- |
|- |
||
|Alumina, AlN |
|Alumina, AlN |
||
Line 81: | Line 80: | ||
|0.5-2 |
|0.5-2 |
||
|} |
|} |
||
+ | |||
+ | === Calculated Blade Exposures === |
||
{| class="wikitable" |
{| class="wikitable" |
||
!Blade Diam |
!Blade Diam |
||
!Flange Diam. |
!Flange Diam. |
||
!Blade Exposure |
!Blade Exposure |
||
+ | ! |
||
|- |
|- |
||
|2.187" (55.55mm) |
|2.187" (55.55mm) |
||
|47mm |
|47mm |
||
|4.275mm |
|4.275mm |
||
⚫ | |||
|- |
|- |
||
|2.187" (55.55mm) |
|2.187" (55.55mm) |
||
|49mm |
|49mm |
||
|3.275mm |
|3.275mm |
||
⚫ | |||
|- |
|- |
||
|2.187" (55.55mm) |
|2.187" (55.55mm) |
||
|51mm |
|51mm |
||
|2.275mm |
|2.275mm |
||
+ | |''51mm Currently Unavailable'' |
||
|- |
|- |
||
|2.187" (55.55mm) |
|2.187" (55.55mm) |
||
|52mm |
|52mm |
||
|1.775mm |
|1.775mm |
||
⚫ | |||
|- |
|- |
||
|2.187" (55.55mm) |
|2.187" (55.55mm) |
||
|53mm |
|53mm |
||
|1.275mm |
|1.275mm |
||
⚫ | |||
|} |
|} |
||
⚫ | |||
− | |||
=== Mounting/Unmounting Samples === |
=== Mounting/Unmounting Samples === |
||
The UV-Release Tape dispenser is most-often used for mounting sample for dicing. |
The UV-Release Tape dispenser is most-often used for mounting sample for dicing. |
||
− | The Tape Model installed is |
+ | The Tape Model installed is Ultron 1042R. [[ADT_UV-Tape_Table_1042R|Data Sheet Here]]. |
− | * Procedure for mounting sample on UV-Release Tape |
+ | * [[ADT WM-966 - UV Tape Mounting Standard Procedure|Procedure for mounting sample on UV-Release Tape]] |
* Full Release: 60 sec exposure |
* Full Release: 60 sec exposure |
||
* Partial Release for Shipping: 9 sec exposure |
* Partial Release for Shipping: 9 sec exposure |
||
=== Surface Protection === |
=== Surface Protection === |
||
+ | |||
+ | ==== Photoresist ==== |
||
Users most often use sacrificial photoresists to protect the surface from accumulating dicing dust. The static-buildup of dielectric films causes the dust to adhere strongly. Ensure that the PR thickness will adequately coat all your exposed topography (eg. use a ≥2µm thick PR for protecting 1.5-2.0µm tall etched features). |
Users most often use sacrificial photoresists to protect the surface from accumulating dicing dust. The static-buildup of dielectric films causes the dust to adhere strongly. Ensure that the PR thickness will adequately coat all your exposed topography (eg. use a ≥2µm thick PR for protecting 1.5-2.0µm tall etched features). |
||
− | # Choose a photoresist of appropriate thickness, and spin-coat it & soft-bake it according to a standard recipe. |
+ | # Choose a photoresist of appropriate thickness, and spin-coat it & soft-bake it according to a standard recipe. |
+ | ## [[Contact Alignment Recipes|Contact Alignment PR Recipes]] |
||
+ | ## [[Stepper Recipes|Stepper PR Recipes]] |
||
# Perform your dicing |
# Perform your dicing |
||
− | # |
+ | # Remove the die from the UV release tape (60sec UV Exposure) |
+ | # Strip the PR from each die in Acetone and ISO & N2 dry |
||
+ | |||
+ | ==== Blue Tape ==== |
||
+ | Alternatively our low-tack residue-free Blue tape can be used to protect the die surface. Blue tape removal is easy for large die, but does require manual removal from each die, and eliminates sample exposure to solvents. |
||
+ | |||
+ | The very edges of the die may accumulate a bit more dicing dust due to the tape delaminating slightly during dicing. Plan for about 50-100µm of edge clearance on each die. |
||
== [[Wafer Bonder (Logitech WBS7)]] == |
== [[Wafer Bonder (Logitech WBS7)]] == |
||
This tool is used for bonding samples to Silicon carrier wafers with CrystalBond wax. |
This tool is used for bonding samples to Silicon carrier wafers with CrystalBond wax. |
||
+ | * [[Logitech WBS7 - Procedure for Wax Mounting with bulk Crystalbond Stick|Wax Mounting Procedure, with bulk Crystalbond Wax]] |
||
+ | * [[Logitech WBS7 - Procedure for Wax Mounting with Spin-On Crystalbond|Wax Mounting Procedure, with Spin-On Crystalbond]] |
||
⚫ | |||
⚫ | |||
− | === Wax Mounting Procedure, with Spin-On Crystalbond === |
||
− | Draft only - in progress. -- Demis 2018-10-16 |
||
− | * Mix a fresh squirt bottle of CrystalBond diluted with Acetone (see [[Don Freeborn]] for method). |
||
− | ** XYZ grams of crystalbond, mixed into |
||
− | ** XYZ mL of Acetone, in dedicated squirt bottle |
||
− | ** Shake/stir to completely dissolve the wax |
||
− | * Place 4-inch silicon carrier wafer on POLOS spinner in solvent bench, with non-vacuum 4-inch chuck installed. |
||
− | * Set up POLOS recipe |
||
− | ** Spin at XYZ rpm for XYZ sec. |
||
− | * Squirt wax solution onto wafer |
||
− | * I/O to spin. |
||
− | * Place carrier wafer on Logitech bonder surface |
||
− | * Place sample to be bonded on top |
||
− | * Place 110mm chemical filter paper on top |
||
− | * Close lid, secure lid clamp |
||
− | * Run recipe: |
||
− | ** XYZ °C |
||
− | ** XYZ seconds |
||
− | ** Vacuum etc.? |
Revision as of 16:08, 14 October 2019
Dicing Saw Recipes (ADT 7100)
Recommended Dicing Parameters
This table is for our stocked Resnoid blades: -4C blades are 4mils/100µm wide, while -8C blades are 8mils/200µm wide. Plan for ~50–100µm extra edge clearance to account for chipping etc.
Narrower (~30-50µm) Nickel Hubbed blades are often used for even narrower dicing streets, these must be purchased by the user.
Material | Blade P/N | Spindle Speed
(KRPM) |
Cut Speed
(mm/s) |
---|---|---|---|
Alumina, AlN | 2.187-8C-54RU-3 | 25 | 0.5-2 |
Ceramic | 2.187-4C-30RU-3 | 18 | 0.5-2 |
GaAs | 2.187-4C-9RU-3 | 35 | 1-5 |
GaN (<550um) | 2.187-4C-30RU-3 | 35 | 0.5-3 |
GaN (>550um) | 2.187-8C-30RU-3 | 35 | 0.5-2 |
Glass/Fused Silica | 2.187-4C-22RU-3 | 25 | 1-5 |
InP | 2.187-4C-9RU-3 | 35 | 1-5 |
Quartz | 2.187-4C-30RU-3 | 25 | 1-5 |
Sapphire | 2.187-8C-54RU-3 | 18 | 0.5-2 |
Si | 2.187-4C-9RU-3 | 35 | 4-10 |
Si on Glasss | 2.187-4C-9RU-3 | 25 | 1-5 |
SiC | 2.187-8C-30RU-3 | 25 | 0.5-2 |
Ti | 2.187-8C-54RU-3 | 15 | 0.5-2 |
Calculated Blade Exposures
Blade Diam | Flange Diam. | Blade Exposure | |
---|---|---|---|
2.187" (55.55mm) | 47mm | 4.275mm | |
2.187" (55.55mm) | 49mm | 3.275mm | |
2.187" (55.55mm) | 51mm | 2.275mm | 51mm Currently Unavailable |
2.187" (55.55mm) | 52mm | 1.775mm | |
2.187" (55.55mm) | 53mm | 1.275mm |
Mounting/Unmounting Samples
The UV-Release Tape dispenser is most-often used for mounting sample for dicing.
The Tape Model installed is Ultron 1042R. Data Sheet Here.
- Procedure for mounting sample on UV-Release Tape
- Full Release: 60 sec exposure
- Partial Release for Shipping: 9 sec exposure
Surface Protection
Photoresist
Users most often use sacrificial photoresists to protect the surface from accumulating dicing dust. The static-buildup of dielectric films causes the dust to adhere strongly. Ensure that the PR thickness will adequately coat all your exposed topography (eg. use a ≥2µm thick PR for protecting 1.5-2.0µm tall etched features).
- Choose a photoresist of appropriate thickness, and spin-coat it & soft-bake it according to a standard recipe.
- Perform your dicing
- Remove the die from the UV release tape (60sec UV Exposure)
- Strip the PR from each die in Acetone and ISO & N2 dry
Blue Tape
Alternatively our low-tack residue-free Blue tape can be used to protect the die surface. Blue tape removal is easy for large die, but does require manual removal from each die, and eliminates sample exposure to solvents.
The very edges of the die may accumulate a bit more dicing dust due to the tape delaminating slightly during dicing. Plan for about 50-100µm of edge clearance on each die.
Wafer Bonder (Logitech WBS7)
This tool is used for bonding samples to Silicon carrier wafers with CrystalBond wax.