+ | ==== Historical Particulate Data ==== |
||
− | Note: Software upgrade performed on 2018-10-10. Note any changes in film. |
||
− | *[https://docs.google.com/spreadsheets/d/1a0XrY6HuJ6L9niThZYI-u4XH69Hnbe3jkm1qKmrR8Rg/edit#gid=sharing Particulates (Gain4) in PECVD#1 2015] |
||
− | *[https://docs.google.com/spreadsheets/d/1ZfkspbCQZmdThC8qB4XyjsyPAzrMF1QbHSMFmH6xSo4/edit#gid=sharing Particulates (Gain4) in PECVD#1 2016] |
||
− | *[https://docs.google.com/spreadsheets/d/1YNiof68Veeh08s_NtG5aCWUXW7GWDDU00HAimV_l8_g/edit#gid=sharing Particulates (Gain4) in PECVD#1 2017] |
||
− | |||
+ | *[https://docs.google.com/spreadsheets/d/1a0XrY6HuJ6L9niThZYI-u4XH69Hnbe3jkm1qKmrR8Rg/edit#gid=sharing Particulates(Gain4) in PECVD#1-OLD DATA 2015] |
||
+ | *[https://docs.google.com/spreadsheets/d/1ZfkspbCQZmdThC8qB4XyjsyPAzrMF1QbHSMFmH6xSo4/edit#gid=sharing Particulates(Gain4) in PECVD#1-OLD DATA 2016] |
||
+ | *[https://docs.google.com/spreadsheets/d/1YNiof68Veeh08s_NtG5aCWUXW7GWDDU00HAimV_l8_g/edit#gid=sharing Particulates(Gain4) in PECVD#1-OLD DATA 2017] |
||
*[https://docs.google.com/spreadsheets/d/1VN551M2oXGWX306HDLQXvZIp3kgxEvWffQqMqnc8ISk/edit#gid=sharing Particulates in PECVD#1 films 2017] |
*[https://docs.google.com/spreadsheets/d/1VN551M2oXGWX306HDLQXvZIp3kgxEvWffQqMqnc8ISk/edit#gid=sharing Particulates in PECVD#1 films 2017] |
||
− | *[https://docs.google.com/spreadsheets/d/11c0gQHnattIjVO95aBqiL-zL4DInRFihV-YB54xLT40/edit#gid=sharing Particulates in |
+ | *[https://docs.google.com/spreadsheets/d/11c0gQHnattIjVO95aBqiL-zL4DInRFihV-YB54xLT40/edit#gid=sharing Particulates in PECVD#1 films 2018] |
+ | *[https://docs.google.com/spreadsheets/d/1ct-SSCRxf81W0jupCWzh81n0DBwPv6mwKFMzuWu_0TI/edit#gid=sharing Particulates in PECVD#1 films 2019] |
||
− | == SiN deposition (PECVD #1) == |
||
+ | *[https://docs.google.com/spreadsheets/d/1yks0OgH8rpbYjin_Qr8vpPg8jBiZQRs_PKfyfo-Rqg0/edit#gid=sharing Particulates in PECVD#1 films 2020] |
||
− | *[[media:New PECVD1-SiO2-standard recipe 2014 SiO2 standard recipe.pdf|SiN Standard Recipe]] |
||
+ | *[https://docs.google.com/spreadsheets/d/1vSmymaS_NNXW-ouC8Ky1J6iVSla7uyRB2zf1lGMa31g/edit#gid=sharing Particulates in PECVD#1 films 2021] |
||
+ | |||
+ | ==SiN deposition (PECVD #1)== |
||
+ | |||
+ | *[https://docs.google.com/spreadsheets/d/1DGU745SeunYz4sLs1LpGKbtOYX-tQyBHEvVYcMxHRKE/edit#gid= Si3N4 Standard Recipe] |
||
+ | ==== Historical Data ==== |
||
+ | |||
+ | ===== Thin-Film Properties ===== |
||
+ | |||
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dEN6LV93LXlnbUhIWU1adVZWMWlXYnc&usp=drive_web#gid=sharing SiN 100nm Data 2014] |
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dEN6LV93LXlnbUhIWU1adVZWMWlXYnc&usp=drive_web#gid=sharing SiN 100nm Data 2014] |
||
*[https://docs.google.com/spreadsheets/d/1phx1WficlUEg0xSahaAq4zrRk6m9Eb0ausO8wcAmXqs/edit#gid=sharing SiN 100nm Data 2015] |
*[https://docs.google.com/spreadsheets/d/1phx1WficlUEg0xSahaAq4zrRk6m9Eb0ausO8wcAmXqs/edit#gid=sharing SiN 100nm Data 2015] |
||
Line 17: | Line 25: | ||
*[https://docs.google.com/spreadsheets/d/1UlyvPcXUBQ5R2JwjKOjELvtCJaTElVhJHfzgjyaRd2A/edit#gid=sharing SiN 300nm Data 2017] |
*[https://docs.google.com/spreadsheets/d/1UlyvPcXUBQ5R2JwjKOjELvtCJaTElVhJHfzgjyaRd2A/edit#gid=sharing SiN 300nm Data 2017] |
||
*[https://docs.google.com/spreadsheets/d/1pAoTCaNSf0uZMyiQ2qKFd0s_e4e53P9Z1jUwtmTnlLk/edit#gid=sharing SiN 300nm Data 2018] |
*[https://docs.google.com/spreadsheets/d/1pAoTCaNSf0uZMyiQ2qKFd0s_e4e53P9Z1jUwtmTnlLk/edit#gid=sharing SiN 300nm Data 2018] |
||
+ | *[https://docs.google.com/spreadsheets/d/1Pnw8eEaQ0rGblRYl6LeIm6wrh1hgeyjnHEbA4BzV8JM/edit#gid=sharing SiN 300nm Data 2019] |
||
+ | *[https://docs.google.com/spreadsheets/d/1N_1Kk6J-wA4nlHpFg5EMDZNHR1kLDo_fr_Dvc6osSr4/edit#gid=sharing SiN 300nm Data 2020] |
||
+ | *[https://docs.google.com/spreadsheets/d/13jY5T_PW1a3GjHIbR0GuUbIhmxClQfvLgzaUtl3YniE/edit#gid=sharing SiN 300nm Data 2021] |
||
+ | ===== Uniformity Data ===== |
||
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dElmTXZyOEZsOFdrMVhNLWpKXzVmNWc&usp=sharing SiN 100 nm Thickness uniformity 2014] |
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dElmTXZyOEZsOFdrMVhNLWpKXzVmNWc&usp=sharing SiN 100 nm Thickness uniformity 2014] |
||
Line 25: | Line 37: | ||
*[https://docs.google.com/spreadsheets/d/1Z83RCH5cAUfViO6vv6hAatcLVWZ95ex4nDdfffm9I7s/edit#gid=sharing SiN 300nm Thickness uniformity 2017] |
*[https://docs.google.com/spreadsheets/d/1Z83RCH5cAUfViO6vv6hAatcLVWZ95ex4nDdfffm9I7s/edit#gid=sharing SiN 300nm Thickness uniformity 2017] |
||
*[https://docs.google.com/spreadsheets/d/1b4EQZdRtVbqNwGBrItoG5-tz6RIzlsvBiCFR6ZXfylw/edit#gid=sharing SiN 300nm Thickness uniformity 2018] |
*[https://docs.google.com/spreadsheets/d/1b4EQZdRtVbqNwGBrItoG5-tz6RIzlsvBiCFR6ZXfylw/edit#gid=sharing SiN 300nm Thickness uniformity 2018] |
||
+ | *[https://docs.google.com/spreadsheets/d/1-OiaH8frAzJzHKfbYTJP808ddzk1Wsv_CixDzG-sSfo/edit#gid=sharing SiN 300nm Thickness uniformity 2019] |
||
+ | *[https://docs.google.com/spreadsheets/d/1e5ycwODa-VooEzGjhY4XquvJpuAuIQHHHZSRwZaH5-E/edit#gid=sharing SiN 300nm Thickness uniformity 2020] |
||
+ | *[https://docs.google.com/spreadsheets/d/1Re5xwB5WMgsgDHsi_0dUeL62uWAnqDQtoBoaR7lj8cI/edit#gid=sharing SiN 300nm Thickness uniformity 2021] |
||
+ | |||
+ | ==SiO<sub>2</sub> deposition (PECVD #1)== |
||
+ | *[https://docs.google.com/spreadsheets/d/1uqpg3sirsRbXdTFlxZ6_k3t0ovP0MtpFtICjpH0-prs/edit#gid= SiO2 Standard Recipe] |
||
+ | |||
+ | ==== Historical Data ==== |
||
+ | |||
+ | ===== Thin-Film Properties ===== |
||
− | == SiO<sub>2</sub> deposition (PECVD #1) == |
||
− | *[[media:New PECVD1-SiN-standard recipe 2014 SiN standard recipe.pdf|SiO<sub>2</sub> Standard Recipe]] |
||
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dEw0bjFEdTF2SUhRa25Ca0d0SzBha3c&usp=drive_web#gid=sharing SiO<sub>2</sub> 100nm Data 2014] |
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dEw0bjFEdTF2SUhRa25Ca0d0SzBha3c&usp=drive_web#gid=sharing SiO<sub>2</sub> 100nm Data 2014] |
||
*[https://docs.google.com/spreadsheets/d/1JWNUcH8l90xif-0BhYKJee9nXxE4hnvvp6N2NtZLYXY/edit#gid=sharing SiO<sub>2</sub> 100nm Data 2015] |
*[https://docs.google.com/spreadsheets/d/1JWNUcH8l90xif-0BhYKJee9nXxE4hnvvp6N2NtZLYXY/edit#gid=sharing SiO<sub>2</sub> 100nm Data 2015] |
||
Line 34: | Line 54: | ||
*[https://docs.google.com/spreadsheets/d/15SocIqWQvBKSvT5oCWoZAURLaaqb9KosxCN2rueZQN8/edit#gid=sharing SiO<sub>2</sub> 300nm Data 2017] |
*[https://docs.google.com/spreadsheets/d/15SocIqWQvBKSvT5oCWoZAURLaaqb9KosxCN2rueZQN8/edit#gid=sharing SiO<sub>2</sub> 300nm Data 2017] |
||
*[https://docs.google.com/spreadsheets/d/1DdjIRGsfJ7WCrxQoGpmzkjLGJhpBTFNYLFmmHcNjAjk/edit#gid=sharing SiO<sub>2</sub> 300nm Data 2018] |
*[https://docs.google.com/spreadsheets/d/1DdjIRGsfJ7WCrxQoGpmzkjLGJhpBTFNYLFmmHcNjAjk/edit#gid=sharing SiO<sub>2</sub> 300nm Data 2018] |
||
+ | *[https://docs.google.com/spreadsheets/d/1QbhukSuVNueT067IVEpweSlD4B7GQecf-tfQFQeV6Xs/edit#gid=sharing SiO<sub>2</sub> 300nm Data 2019] |
||
+ | *[https://docs.google.com/spreadsheets/d/1OwyhfFPDH-XLPczA8cKoBPnujq9oNukaWkHq0KoFS40/edit#gid=sharing SiO<sub>2</sub> 300nm Data 2020] |
||
+ | *[https://docs.google.com/spreadsheets/d/1I-0Ih_F9pWeOwXeEQC6IFYKNB6bBLSoBiyX8Eu3pwFg/edit#gid=sharing SiO<sub>2</sub> 300nm Data 2021] |
||
+ | ===== Thick-Film Properties ===== |
||
+ | *[https://docs.google.com/spreadsheets/d/1XgUlCaCv3jCK9RyrI553PkIS0PmiAlbWjsDwK5TOH3I/edit#gid=sharing SiO<sub>2</sub> Thick film Data 2021] |
||
+ | ==== Uniformity Data ==== |
||
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dDQ3VEtZQVRpdVdlbGtIZHpTNmFzNmc&usp=drive_web#gid=sharing SiO<sub>2</sub> 100nm Thickness uniformity 2014] |
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dDQ3VEtZQVRpdVdlbGtIZHpTNmFzNmc&usp=drive_web#gid=sharing SiO<sub>2</sub> 100nm Thickness uniformity 2014] |
||
Line 43: | Line 69: | ||
*[https://docs.google.com/spreadsheets/d/1Fa8mZIBIeJwvCwUbJ-28VcvVYj8rshhuDuXsYxA-cD8/edit#gid=sharing SiO<sub>2</sub> 300nm Thickness uniformity 2017] |
*[https://docs.google.com/spreadsheets/d/1Fa8mZIBIeJwvCwUbJ-28VcvVYj8rshhuDuXsYxA-cD8/edit#gid=sharing SiO<sub>2</sub> 300nm Thickness uniformity 2017] |
||
*[https://docs.google.com/spreadsheets/d/1YB_9USpuXGpIdSW2gNsptu5nSrLWAGsYu0SWoYEy0aQ/edit#gid=sharing SiO<sub>2</sub> 300nm Thickness uniformity 2018] |
*[https://docs.google.com/spreadsheets/d/1YB_9USpuXGpIdSW2gNsptu5nSrLWAGsYu0SWoYEy0aQ/edit#gid=sharing SiO<sub>2</sub> 300nm Thickness uniformity 2018] |
||
+ | *[https://docs.google.com/spreadsheets/d/1FatUAEegWuDRzVa47L1_cqgRs0AZ_Fao9jpwz5sfln0/edit#gid=sharing SiO<sub>2</sub> 300nm Thickness uniformity 2019] |
||
+ | *[https://docs.google.com/spreadsheets/d/1uAIEv_z2TJtY2XxTYnDIyKwKT4ZIhalTCyZ5SrDRJmA/edit#gid=sharing SiO<sub>2</sub> 300nm Thickness uniformity 2020] |
||
+ | *[https://docs.google.com/spreadsheets/d/1jThamYtEiH3lVz4IzoG9ILxBG8-TufIKnUd8V0qKQU0/edit#gid=sharing SiO<sub>2</sub> 300nm Thickness uniformity 2021] |
||
− | == |
+ | == Low-Stress SiN - LS-SiN (PECVD#1) == |
+ | |||
− | <!-- Placeholders - Not uploaded yet--> |
||
− | *[ |
+ | *[//wiki.nanotech.ucsb.edu/wiki/images/4/4a/New_PECVD1-LS_SIN-Turner05recipe_2014_LS_SIN_recipe.pdf LS SiN Standard Recipe] |
*[https://docs.google.com/spreadsheets/d/1Joz0az9TGZWQc4CiMQJZzLBbNFbx_hH2Oc0B4NNJmYk/edit#gid=sharing LS SiN Data 2014] |
*[https://docs.google.com/spreadsheets/d/1Joz0az9TGZWQc4CiMQJZzLBbNFbx_hH2Oc0B4NNJmYk/edit#gid=sharing LS SiN Data 2014] |
||
*[https://docs.google.com/spreadsheets/d/1xIzc2CufRYNSfAtsOXpw3IzHreeu42BWrLBV0kzP6kA/edit#gid=sharing LS SiN 1000A Thickness uniformity 2014] |
*[https://docs.google.com/spreadsheets/d/1xIzc2CufRYNSfAtsOXpw3IzHreeu42BWrLBV0kzP6kA/edit#gid=sharing LS SiN 1000A Thickness uniformity 2014] |
||
+ | |||
− | *[[media:New PECVD1-LS SION-recipe 2014 LS SION recipe.pdf|SiO<sub>x</sub>N<sub>y</sub> Standard Recipe]] |
||
+ | == SiO<sub>x</sub>N<sub>y</sub> deposition (PECVD #1) == |
||
+ | |||
+ | *[//wiki.nanotech.ucsb.edu/wiki/images/2/24/New_PECVD1-LS_SION-recipe_2014_LS_SION_recipe.pdf SiO<sub>x</sub>N<sub>y</sub> Standard Recipe] |
||
*[https://docs.google.com/spreadsheets/d/1rixyzAAq6q08M5OwvZiDVoh3K8B566XKM-UZAQIAnsg/edit#gid=sharing SiO<sub>x</sub>N<sub>y</sub> Data 2014] |
*[https://docs.google.com/spreadsheets/d/1rixyzAAq6q08M5OwvZiDVoh3K8B566XKM-UZAQIAnsg/edit#gid=sharing SiO<sub>x</sub>N<sub>y</sub> Data 2014] |
||
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dEttR2JSTkRoamR0SUZ4bE5QUW9uS2c&usp=sharing SiO<sub>x</sub>N<sub>y</sub>1000A Thickness uniformity 2014] |
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dEttR2JSTkRoamR0SUZ4bE5QUW9uS2c&usp=sharing SiO<sub>x</sub>N<sub>y</sub>1000A Thickness uniformity 2014] |
||
+ | |||
+ | == Cleaning Recipes (PECVD #1) == |
||
+ | The cleaning procedure is very important in order to have consistent result on this tool and also to keep particulate count low. After each deposition you should clean the tool following instructions carefully. The clean is done in two steps: |
||
+ | # Wet cleaning (start cleaning by using a cleanroom wipe sprayed with DI. Wipe chamber sidewalls with it. Finish cleaning by using the cleanroom wipe sprayed with IPA. ) |
||
+ | # Load the recipe for cleaning "CF4/O2 Clean" (edit the recipe and change ONLY time of cleaning). Follow instructions regarding a required time for cleaning. |
||
+ | |||
+ | === [//wiki.nanotech.ucsb.edu/w/images/7/72/PECVD1-cleaning.png Standard Cleaning Recipe: "CF4/O2 Clean"] === |
||
+ | Click the above link for a screenshot of the standard cleaning recipe, for which you will enter a custom time. The recipe is set up so that it will '''pop up a window for the cleaning time upon running the recipe''' - you do not need to edit the recipe before running it. |
||
=[[PECVD 2 (Advanced Vacuum)]]= |
=[[PECVD 2 (Advanced Vacuum)]]= |
||
+ | |||
+ | ==== Historical Particulate Data ==== |
||
+ | |||
*[https://docs.google.com/spreadsheets/d/1kj0SWxRpnPRoGld8k3sW-3yK1iPm3buTkvlJSN5YPV4/edit#gid=sharing Particulates (Gain4) in PECVD#2 2015] |
*[https://docs.google.com/spreadsheets/d/1kj0SWxRpnPRoGld8k3sW-3yK1iPm3buTkvlJSN5YPV4/edit#gid=sharing Particulates (Gain4) in PECVD#2 2015] |
||
*[https://docs.google.com/spreadsheets/d/1xpk9tJrE68NIJ_1yIym0xBxd4fnzHHBHdkhFehruO3E/edit#gid=sharing Particulates (Gain4) in PECVD#2 2016] |
*[https://docs.google.com/spreadsheets/d/1xpk9tJrE68NIJ_1yIym0xBxd4fnzHHBHdkhFehruO3E/edit#gid=sharing Particulates (Gain4) in PECVD#2 2016] |
||
Line 60: | Line 103: | ||
*[https://docs.google.com/spreadsheets/d/1yPAPP24z3RcRRi-HqEp3GJN4JM8Ec8SFJwZ-OYGG2HU/edit#gid=sharing Particulates in PECVD#2 films 2017] |
*[https://docs.google.com/spreadsheets/d/1yPAPP24z3RcRRi-HqEp3GJN4JM8Ec8SFJwZ-OYGG2HU/edit#gid=sharing Particulates in PECVD#2 films 2017] |
||
*[https://docs.google.com/spreadsheets/d/1aU6fTyQ5MlGD4uCa9gepG5rLJzW3wlkOWSKEl_w_Ye4/edit#gid=sharing Particulates in PECVD#2 films 2018] |
*[https://docs.google.com/spreadsheets/d/1aU6fTyQ5MlGD4uCa9gepG5rLJzW3wlkOWSKEl_w_Ye4/edit#gid=sharing Particulates in PECVD#2 films 2018] |
||
− | *[https://docs.google.com/spreadsheets/d/ |
+ | *[https://docs.google.com/spreadsheets/d/1OPZXe8g3H0wywIrPFel3nSZ5iyPs2mVIYUSVKfTtMDg/edit#gid=sharing Particulates in PECVD#2 films 2019] |
+ | *[https://docs.google.com/spreadsheets/d/1Y9lomsf7bDojeXoAsEG7xvypx_sw_atpmPwB9xtK1Zk/edit#gid=sharing Particulates in PECVD#2 films 2020] |
||
− | == SiO<sub>2</sub> deposition (PECVD #2) == |
||
+ | *[https://docs.google.com/spreadsheets/d/1BauS7q_sGKkaeY6o3BOw2wyQsyS_DukJxCAbGantDW4/edit#gid=sharing Particulates in PECVD#2 films 2021] |
||
+ | |||
+ | ==SiO<sub>2</sub> deposition (PECVD #2)== |
||
+ | |||
+ | ==== Standard Recipe ==== |
||
+ | |||
+ | |||
+ | *[https://docs.google.com/spreadsheets/d/1wCEcFj6ZMHR4QifngLXwz6dqbyf8hsVKu7bQbMS6EoA/edit#gid= STD SiO2 Recipe] |
||
+ | |||
+ | ==== Historical Data ==== |
||
+ | |||
+ | ===== Thin-Film Properties ===== |
||
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dGJZaGtDTVRqa1BRdW5iU1N1Y01jd0E&usp=drive_web#gid=sharing Oxide Data 2014] |
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dGJZaGtDTVRqa1BRdW5iU1N1Y01jd0E&usp=drive_web#gid=sharing Oxide Data 2014] |
||
Line 68: | Line 123: | ||
*[https://docs.google.com/spreadsheets/d/1vcaHwraMGNHuRxgWwGp78EJf4T3Jk182wxoCz_neuck/edit#gid=sharing Oxide Data 2017] |
*[https://docs.google.com/spreadsheets/d/1vcaHwraMGNHuRxgWwGp78EJf4T3Jk182wxoCz_neuck/edit#gid=sharing Oxide Data 2017] |
||
*[https://docs.google.com/spreadsheets/d/1VI-sUmaqois0NsCvf2kQmPfRRa03MjBzl779hmmLtP4/edit#gid=sharing Oxide Data 2018] |
*[https://docs.google.com/spreadsheets/d/1VI-sUmaqois0NsCvf2kQmPfRRa03MjBzl779hmmLtP4/edit#gid=sharing Oxide Data 2018] |
||
− | *[https://docs.google.com/spreadsheets/d/ |
+ | *[https://docs.google.com/spreadsheets/d/1oWnQ3D6oknKWU2bohvSrN85rlEZgQN3YP_ZJ4i8u7do/edit#gid=sharing Oxide Data 2019] |
+ | *[https://docs.google.com/spreadsheets/d/1Z9UMgaQC2PiLLrMk04mpKWkJLa1L_WFMAm5079eKxI0/edit#gid=sharing Oxide Data 2020] |
||
+ | *[https://docs.google.com/spreadsheets/d/10XA3WnHjUZOLFunwUIlM2IqaRIiX_EGb6Jj_bw84gkI/edit#gid=sharing Oxide Data 2021] |
||
+ | |||
+ | ===== Thin-Film Properties ===== |
||
+ | *[https://docs.google.com/spreadsheets/d/19Z8IAVgumWuH0t8RN23LJ2wWZP7jYYLwRl9pDQP4obI/edit#gid=sharing Thick Oxide Data 2021] |
||
+ | |||
+ | ===== Uniformity Data ===== |
||
+ | |||
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dDRjSHEtYUZRUTg4azE2U0JGUTg2M1E#gid=sharing Oxide Thickness Uniformity 2014] |
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dDRjSHEtYUZRUTg4azE2U0JGUTg2M1E#gid=sharing Oxide Thickness Uniformity 2014] |
||
*[https://docs.google.com/spreadsheets/d/16pZHcGwesXB1mMPwntOudBIlPvRh6A6DI37DEwyYfPw/edit#gid=sharing Oxide Thickness Uniformity 2015] |
*[https://docs.google.com/spreadsheets/d/16pZHcGwesXB1mMPwntOudBIlPvRh6A6DI37DEwyYfPw/edit#gid=sharing Oxide Thickness Uniformity 2015] |
||
Line 75: | Line 138: | ||
*[https://docs.google.com/spreadsheets/d/1064j6894X63WlRX3Uolxg1q1FRzUZLqSZQA9BWwzPOk/edit#gid=sharing Oxide Thickness Uniformity 2018] |
*[https://docs.google.com/spreadsheets/d/1064j6894X63WlRX3Uolxg1q1FRzUZLqSZQA9BWwzPOk/edit#gid=sharing Oxide Thickness Uniformity 2018] |
||
*[https://docs.google.com/spreadsheets/d/1064j6894X63WlRX3Uolxg1q1FRzUZLqSZQA9BWwzPOk/edit#gid=sharing Oxide Thickness Uniformity 2019] |
*[https://docs.google.com/spreadsheets/d/1064j6894X63WlRX3Uolxg1q1FRzUZLqSZQA9BWwzPOk/edit#gid=sharing Oxide Thickness Uniformity 2019] |
||
+ | *[https://docs.google.com/spreadsheets/d/1Z9UMgaQC2PiLLrMk04mpKWkJLa1L_WFMAm5079eKxI0/edit#gid=sharing Oxide Thickness Uniformity 2020] |
||
+ | *[https://docs.google.com/spreadsheets/d/1b9Fmzp_d-XiMerFtrDiCsmS7NMNoaBtS8T0DLqoii8Y/edit#gid=sharing Oxide Thickness Uniformity 2021] |
||
+ | ==SiN deposition (PECVD #2)== |
||
+ | ==== Standard Recipe ==== |
||
− | *[[media:New Adv PECVD OXIDE 300C standard recipe OXIDE Standard Recipe.pdf|Oxide Standard Recipe 2014-5/9/18]] |
||
− | *[[media:STD SiO2 5-9-18.pdf|STD SiO2 5/9/18]] |
||
+ | *[//wiki.nanotech.ucsb.edu/wiki/images/4/4c/SiNx_Films_by_PECVD2.pdf SiNx Film Stress vs LF and HF Duration Time, and Gas Flowing-rate] |
||
− | == SiN deposition (PECVD #2) == |
||
+ | *[https://docs.google.com/spreadsheets/d/1KS4HfhUJyYVep4H6CRAKpMRP5TA31F0qD-obQkKRnEI/edit#gid= STD Nitride2 Recipe] |
||
+ | |||
+ | ==== Historical Data ==== |
||
+ | |||
+ | ===== Thin-Film Properties ===== |
||
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dDE0R3FlenNPa2txNmRldTczMXZNNnc#gid=sharing Nitride2 Data 2014] |
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dDE0R3FlenNPa2txNmRldTczMXZNNnc#gid=sharing Nitride2 Data 2014] |
||
Line 87: | Line 157: | ||
*[https://docs.google.com/spreadsheets/d/1f3JBEnr7lf0yIMlzlOYKv_bXlIDyXt8vec_rSVJIoOk/edit#gid=sharing Nitride2 Data 2017] |
*[https://docs.google.com/spreadsheets/d/1f3JBEnr7lf0yIMlzlOYKv_bXlIDyXt8vec_rSVJIoOk/edit#gid=sharing Nitride2 Data 2017] |
||
*[https://docs.google.com/spreadsheets/d/1OO0ewGSqYSzL3lj8fXkgckTkBGQRliD6sBc02IW7wZY/edit#gid=sharing Nitride2 Data 2018] |
*[https://docs.google.com/spreadsheets/d/1OO0ewGSqYSzL3lj8fXkgckTkBGQRliD6sBc02IW7wZY/edit#gid=sharing Nitride2 Data 2018] |
||
− | *[https://docs.google.com/spreadsheets/d/ |
+ | *[https://docs.google.com/spreadsheets/d/1Zi8CRspd3LTDdNRRCneE0--bVohWvZbV_kSHo04s0oI/edit#gid=sharing Nitride2 Data 2019] |
+ | *[https://docs.google.com/spreadsheets/d/1LEutQynQXU_9B4EqRt21PX9TGR13IqaMge7sKAXKAfg/edit#gid=sharing Nitride2 Data 2020] |
||
+ | *[https://docs.google.com/spreadsheets/d/1piGMPEHXiUV5WMNfaTFKdL1pnE8W2yrWHkNWHd7Au1A/edit#gid=sharing Nitride2 Data 2021] |
||
+ | |||
+ | ===== Uniformity Data ===== |
||
+ | |||
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dERkYm85bGtYQVpjVk5GTGJuMkg2anc&usp=drive_web#gid=sharing Nitride2 Thickness Uniformity 2014] |
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dERkYm85bGtYQVpjVk5GTGJuMkg2anc&usp=drive_web#gid=sharing Nitride2 Thickness Uniformity 2014] |
||
*[https://docs.google.com/spreadsheets/d/14_dYQu3z31fF_oxsUUX8BmDucgv6B07xB3_zqP0HmvM/edit#gid=sharing Nitride2 Thickness Uniformity 2015] |
*[https://docs.google.com/spreadsheets/d/14_dYQu3z31fF_oxsUUX8BmDucgv6B07xB3_zqP0HmvM/edit#gid=sharing Nitride2 Thickness Uniformity 2015] |
||
Line 94: | Line 169: | ||
*[https://docs.google.com/spreadsheets/d/1hzj4Fb5fN8lS0m9-rm9AgEn0Zunif5grI4X7YkAMEFU/edit#gid=sharing Nitride2 Thickness Uniformity 2018] |
*[https://docs.google.com/spreadsheets/d/1hzj4Fb5fN8lS0m9-rm9AgEn0Zunif5grI4X7YkAMEFU/edit#gid=sharing Nitride2 Thickness Uniformity 2018] |
||
*[https://docs.google.com/spreadsheets/d/1hzj4Fb5fN8lS0m9-rm9AgEn0Zunif5grI4X7YkAMEFU/edit#gid=sharing Nitride2 Thickness Uniformity 2019] |
*[https://docs.google.com/spreadsheets/d/1hzj4Fb5fN8lS0m9-rm9AgEn0Zunif5grI4X7YkAMEFU/edit#gid=sharing Nitride2 Thickness Uniformity 2019] |
||
+ | *[https://docs.google.com/spreadsheets/d/1xdzjLODpe2Xb7r4PGil1q-OFqSYKuZBivqLt1T6lezw/edit#gid=sharing Nitride2 Thickness Uniformity 2020] |
||
+ | *[https://docs.google.com/spreadsheets/d/19x70-CIyQ41pywpL-IusldLv7XYJps9aJT5-rYYQSCs/edit#gid=sharing Nitride2 Thickness Uniformity 2021] |
||
+ | ==Low-Stress SiN deposition (PECVD #2)== |
||
+ | ''Low-Stress SilIcon Nitride (< 100 MPa)'' |
||
+ | ==== Standard Recipe ==== |
||
− | *[[media:SiNx Films by PECVD2.pdf|SiNx Film Stress vs LF and HF Duration Time, and Gas Flowing-rate]] |
||
+ | *[https://docs.google.com/spreadsheets/d/1DzzI7aE61R7c6gyk6cGBdm9FtGrApiNJ4AL90ll2C8k/edit#gid= STD LS Nitride2 Recipe] |
||
+ | *''Old Versions:'' |
||
+ | **[//wiki.nanotech.ucsb.edu/wiki/images/a/a5/New_AdvPECVD-LS_Nitride2_300C_standard_recipe_LS_Nitride2_standard_recipe.pdf LS Nitride2 Standard Recipe 2014-5/9/2018] |
||
+ | **[//wiki.nanotech.ucsb.edu/wiki/images/0/01/STD_LSNitride2_5-9-18.pdf STD LSNitride2 5/9/2018] |
||
+ | ==== Historical Data ==== |
||
− | *[[media:New Adv PECVD-Nitride2 300C standard recipe Nitride2 Standard Recipe.pdf|Nitride2 Standard Recipe 2014-5/9/2018]] |
||
− | *[[media:STD Nitride 5-9-18 Dep.recipe.pdf|STD Nitride2 Standard Recipe 5/9/2018]] |
||
+ | ===== Thin-Film Properties ===== |
||
− | ==Low-Stress SiN deposition (PECVD #2) == |
||
− | Low-Stress SilIcon Nitride (< 100 MPa) |
||
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dEZvWVhzS1pHUXZkOGcyQWZ4LTNBWGc&usp=drive_web#gid=sharing LS Nitride2 Data 2014] |
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dEZvWVhzS1pHUXZkOGcyQWZ4LTNBWGc&usp=drive_web#gid=sharing LS Nitride2 Data 2014] |
||
Line 111: | Line 192: | ||
*[https://docs.google.com/spreadsheets/d/1vwpDtiglR2DLWiYNhpBX77cyyj9lw55iVeFz1puN7bM/edit#gid=sharing LS Nitride2 Data 2018] |
*[https://docs.google.com/spreadsheets/d/1vwpDtiglR2DLWiYNhpBX77cyyj9lw55iVeFz1puN7bM/edit#gid=sharing LS Nitride2 Data 2018] |
||
*[https://docs.google.com/spreadsheets/d/1zvSl2P5T926Ol48yH3FBCZm1zCeycl3S8GWQYtzi8VI/edit#gid=sharing LS Nitride2 Data 2019] |
*[https://docs.google.com/spreadsheets/d/1zvSl2P5T926Ol48yH3FBCZm1zCeycl3S8GWQYtzi8VI/edit#gid=sharing LS Nitride2 Data 2019] |
||
+ | *[https://docs.google.com/spreadsheets/d/1muyFsIspqZXB2HXiqG3t39uzeO7A7Srvh4aGdXjwCc4/edit#gid=sharing LS Nitride2 Data 2020] |
||
+ | *[https://docs.google.com/spreadsheets/d/1qzVA44esh71655lE1rrpGkKKNTyZRC_mv3IaiZ_HAWQ/edit#gid=sharing LS Nitride2 Data 2021] |
||
+ | |||
+ | ===== Uniformity Data ===== |
||
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dENSak1ZNnVaVTFEQTBzdDJMSDlDTFE&usp=drive_web#gid=1=sharing LS Nitride2 Thickness Uniformity 2014] |
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dENSak1ZNnVaVTFEQTBzdDJMSDlDTFE&usp=drive_web#gid=1=sharing LS Nitride2 Thickness Uniformity 2014] |
||
Line 118: | Line 203: | ||
*[https://docs.google.com/spreadsheets/d/17OGrhbvP8O_0mBMIsmUmEwfyFaoJnNNpMFpgBUW7qzI/edit#gid=sharing LS Nitride2 Thickness Uniformity 2018] |
*[https://docs.google.com/spreadsheets/d/17OGrhbvP8O_0mBMIsmUmEwfyFaoJnNNpMFpgBUW7qzI/edit#gid=sharing LS Nitride2 Thickness Uniformity 2018] |
||
*[https://docs.google.com/spreadsheets/d/17OGrhbvP8O_0mBMIsmUmEwfyFaoJnNNpMFpgBUW7qzI/edit#gid=sharing LS Nitride2 Thickness Uniformity 2019] |
*[https://docs.google.com/spreadsheets/d/17OGrhbvP8O_0mBMIsmUmEwfyFaoJnNNpMFpgBUW7qzI/edit#gid=sharing LS Nitride2 Thickness Uniformity 2019] |
||
+ | *[https://docs.google.com/spreadsheets/d/1M4ug8SAqy2Ky70LNLW3pL2MjSs69beJVhbC2BbabHaU/edit#gid=sharing LS Nitride2 Thickness Uniformity 2020] |
||
+ | *[https://docs.google.com/spreadsheets/d/12wvXFHN7CV_XSFj6hB5Gd7SIXERwzkTM__58ZqzPOuk/edit#gid=sharing LS Nitride2 Thickness Uniformity 2021] |
||
+ | |||
+ | ==Amorphous-Si deposition (PECVD #2)== |
||
+ | *[//wiki.nanotech.ucsb.edu/wiki/images/9/9d/03-Amorphous-Si-PECVD-2.pdf Amorphous Si Deposition Recipe] |
||
+ | *[//wiki.nanotech.ucsb.edu/wiki/images/0/09/ASi_deposition_and_film_stress_using_AV_dep_tool.pdf Amorphous Si Films and Their Stress] |
||
+ | == Cleaning Recipes (PECVD #2) == |
||
+ | The cleaning procedure is very important in order to have consistent result on this tool and also to keep particulate count low. After each deposition you should clean the tool following instructions carefully. The clean is done in two steps: |
||
+ | #Wet cleaning (start cleaning by using a cleanroom wipe sprayed with DI. Wipe chamber sidewalls with it. Finish cleaning by using the cleanroom wipe sprayed with IPA. ) |
||
+ | #Load the recipe for cleaning "STD CF4/O2 Clean" (edit the recipe and change ONLY time of cleaning). Follow instructions regarding a required time for cleaning. |
||
+ | ===[//wiki.nanotech.ucsb.edu/w/images/3/34/PECVD2_photo_for_cleaning.png Standard Clean Recipe: "STD CF4/O2 Clean recipe"] === |
||
+ | Click the above link for a screenshot of the standard cleaning recipe, for which you will enter a custom time. The recipe is set up so that it will '''pop up a window for the cleaning time upon running the recipe''' - you do not need to edit the recipe before running it. |
||
+ | =[[ICP-PECVD (Unaxis VLR)]]= |
||
− | *[[media:New AdvPECVD-LS Nitride2 300C standard recipe LS Nitride2 standard recipe.pdf|LS Nitride2 Standard Recipe 2014-5/9/2018]] |
||
+ | 2020-02: New recipes have been characterized for low particulate count and repeatability. Only staff-supplied recipes are allowed in the tool. Please follow the [[ICP-PECVD (Unaxis VLR)#Documentation|'''new procedures''']] to ensure low particle counts in the chamber. |
||
+ | The system currently has '''Deuterated Silane (SiD<sub>4</sub>) installed''' - identical to the regular Silicon precursor SiH<sub>4</sub>, except that it significantly lowers optical absorption in the near-infrared due to shifted molecular vibrations/molecular weights. |
||
− | *[[media:STD LSNitride2 5-9-18.pdf|STD LSNitride2 5/9/2018]] |
||
+ | ==== Historical Particulate Data ==== |
||
− | *[[media:STD LSNitride2 12-14-18 recipe.pdf|STD LSNitride2 12/14/2018]] |
||
+ | * [https://docs.google.com/spreadsheets/d/1ZzbpDmkOI3IvGuKqyiQIP44sYJ89E3Zs9sLvjxvWMsc/edit#gid=sharing Particulates in Unaxis films @250C-2019] |
||
+ | * [https://docs.google.com/spreadsheets/d/1fMebt-6BfAurcjMv1aDsmm6VgPqokU73_2ReZFqzEEk/edit#gid=sharing Particulates in Unaxis films @250C-2020] |
||
+ | ==== Standard Recipes ==== |
||
− | == Amorphous-Si deposition (PECVD #2) == |
||
+ | *[https://docs.google.com/spreadsheets/d/1T_4gaJQ3wHSNptoAtFR1fN0ePwfw3PsQ0DLSjqGeyM4/edit#gid=sharing SiO2 LDR 250C Recipe-2020] |
||
− | *[[media:03-Amorphous-Si-PECVD-2.pdf|Amorphous Si Deposition Recipe]] |
||
+ | *[https://docs.google.com/spreadsheets/d/1nsdGPpfyZfIesyYG1PIU9uYyuzQWrfpsvVWM6J_H6BI/edit#gid=sharing SiO2 HDR 250C Recipe-2020] |
||
− | *[[media:ASi deposition and film stress using AV dep tool.pdf|Amorphous Si Films and Their Stress]] |
||
+ | *[https://docs.google.com/spreadsheets/d/1UTr93aWx0MjCwVBwRmYjPwo9ASluGQ-OrJhVG_R57aY/edit#gid=sharing SiN 250C Recipe-2020] |
||
+ | *[https://docs.google.com/spreadsheets/d/1MXW7UNpTyk93ucOVQaSun5IX7QaUbSABNHNznb09qw8/edit#gid=sharing SiN LS 250C Recipe-2020] |
||
− | = |
+ | ==SiO2 LDR 250C Deposition (Unaxis VLR)== |
+ | ''Low-Deposition Rate SiO<sub>2</sub>'' |
||
− | ==SiN deposition (Unaxis VLR) == |
||
− | === SiN (2% SiH<sub>4</sub>) === |
||
− | {| class="wikitable" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center;" border="1" |
||
− | |- bgcolor="#D0E7FF" |
||
− | ! width="350" align="center" |50° (pinholes) |
||
− | ! width="350" align="center" |100° (pinholes) |
||
− | ! width="350" align="center" |250° |
||
− | |- align="left" |
||
− | | |
||
− | *[[Media:PECVD2-SiN-Recipe-5W-50C-High-Stress.pdf|SiN Deposition Recipe (5W 50° High Stress)]] |
||
− | *[[Media:PECVD2-SiN-Recipe-50W-50C-Medium-Stress.pdf|SiN Deposition Recipe (50W 50° Medium Stress)]] |
||
− | *[[Media:PECVD2-SiN-Recipe-120W-50C-Low-Stress.pdf|SiN Deposition Recipe (120W 50° Low Stress)]] |
||
− | | |
||
− | *[[Media:PECVD2-SiN-Recipe-5W-100C-High-Stress.pdf|SiN Deposition Recipe (5W 100° High Stress)]] |
||
− | *[[Media:PECVD2-SiN-Recipe-50W-100C-Medium-Stress.pdf|SiN Deposition Recipe (50W 100° Medium Stress)]] |
||
− | *[[Media:PECVD2-SiN-Recipe-120W-100C-Low-Stress.pdf|SiN Deposition Recipe (120W 100° Low Stress)]] |
||
− | *[[Media:PECVD2-SiNx-l.s.-Comparison table-2% SiH4-100C-120W.pdf|Comparison Table SiNx (120W 100° Low Stress)]] |
||
− | *[[Media:PECVD2-SiNx-medium-Comparison table-2% SiH4-100C-120W.pdf|Comparison Table SiNx (50W 100° Medium Stress)]] |
||
− | *[[Media:PECVD2-SiNx -h.s.-Comparison table-2% SiH4-100C-120W.pdf|Comparison Table SiNx (5W 100° High Stress)]] |
||
− | *[[Media:PECVD2-SiNx-medium stress-SEM-2% SiH4-100C-50W.pdf|SiNx SEM images (50W 100° Medium Stress)]] |
||
− | *[[Media:PECVD2-SiNx-high stress-SEM-2% SiH4-100C-5W.pdf|SiNx SEM images (5W 100° High Stress)]] |
||
− | | |
||
− | *[[Media:PECVD2-SiN-Recipe-5W-250C-High-Stress.pdf|SiN Deposition Recipe (5W 250° High Stress)]] |
||
− | *[[Media:PECVD2-SiN-Recipe-50W-250C-Medium-Stress.pdf|SiN Deposition Recipe (50W 250° Medium Stress)]] |
||
− | *[[Media:PECVD2-SiN-Recipe-120W-250C-Low-Stress.pdf|SiN Deposition Recipe (120W 250° Low Stress)]] |
||
− | *[[Media:PECVD2-SiNx-l.s.-Comparison table-2% SiH4-100C-120W.pdf|Comparison Table SiNx (120W 250° Low Stress)]] |
||
− | *[[Media:PECVD2-SiNx-medium-Comparison table-2% SiH4-100C-120W.pdf|Comparison Table SiNx (50W 250° Medium Stress)]] |
||
− | *[[Media:PECVD2-SiNx -h.s.-Comparison table-2% SiH4-100C-120W.pdf|Comparison Table SiNx (5W 250° High Stress)]] |
||
− | *[[Media:28-Very-low-pin-hole-density SiNx film at 300 C.pdf|Very-Low-Pin-Hole-Density SiNx Recipe(25W 300°)]] |
||
− | |- |
||
− | |} |
||
+ | ==== Historical Data ==== |
||
− | === SiN (2% SiH<sub>4</sub> - No-Ar) === |
||
+ | ===== Thin-Film Properties ===== |
||
− | {| class="wikitable" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center;" border="1" |
||
+ | This data is for 780sec long SiO2 LDR (low deposition rate) deposition, and cleaning time is 900sec, following the procedure [[here]]. |
||
− | |- bgcolor="#D0E7FF" |
||
+ | *[https://docs.google.com/spreadsheets/d/1wocoCPOOEDQcZbXJJNaZs1sr9dXBZpn1wUyglL8IQrI/edit#gid=sharing SiO2 LDR 250C 300nm Data-2019] |
||
− | ! width="350" align="center" |50° (pinholes) |
||
+ | *[https://docs.google.com/spreadsheets/d/1bU2Gu3x3DNyrq8skMAQZJCsra-IcoDCT0U5D135YPgc/edit#gid=sharing SiO2 LDR 250C 300nm Data-2020] |
||
− | ! width="350" align="center" |100° (pinholes) |
||
+ | ===== Uniformity Data ===== |
||
− | ! width="350" align="center" |250° |
||
+ | *[https://docs.google.com/spreadsheets/d/1Xi21OrargcNRthZ2fM_56APB8O599ctDfq5E_6B5Ft0/edit#gid=sharing Thickness Uniformity SiO2 LDR 250C 300nm-2019] |
||
− | |- align="left" |
||
+ | *[https://docs.google.com/spreadsheets/d/1-ytu5R75FAXNfhJZTRuK2eRZyu_L6Hy1BWV2zN6_tRA/edit#gid=sharing Thickness Uniformity SiO2 LDR 250C 300nm-2020] |
||
− | | |
||
− | *[[Media:PECVD2-SiN-Recipe-NoAr-5W-50C-High-Stress.pdf|SiN Deposition Recipe - No Ar (5W 50° High Stress)]] |
||
− | *[[Media:41-High-stress SiNx at 50 C using Unaxis ICP deposition tool.pdf|Film Properties of High-stress SiN<sub>x</sub> (No Ar, 5W, 50°)]] |
||
− | *[[Media:PECVD2-SiN-Recipe-NoAr-50W-50C-Medium-Stress.pdf|SiN Deposition Recipe - No Ar (50W 50° Medium Stress)]] |
||
− | *[[Media:36-Medium-stress SiNx using Unaxis ICP deposition tool-a.pdf|Film Properties of Medium-stress SiN<sub>x</sub> (No Ar, 50W, 50°)]] |
||
− | *[[Media:PECVD2-SiN-Recipe-NoAr-120W-50C-Low-Stress.pdf|SiN Deposition Recipe - No Ar (120W 50° Low Stress)]] |
||
− | *[[Media:40-Low-stress SiNx at 50 C using Unaxis ICP deposition tool.pdf|Film Properties of Low-stress SiN<sub>x</sub> (No Ar, 120W, 50°)]] |
||
− | | |
||
− | *[[Media:PECVD2-SiN-Recipe-NoAr-5W-100C-High-Stress.pdf|SiN Deposition Recipe - No Ar (5W 100° High Stress)]] |
||
− | *[[Media:38-High-stress SiNx at 100 C using Unaxis ICP deposition tool.pdf|Film Properties of high-stress SiN<sub>x</sub> (No Ar, 5W, 100°)]] |
||
− | *[[Media:PECVD2-SiN-Recipe-NoAr-50W-100C-Medium-Stress.pdf|SiN Deposition Recipe - No Ar (50W 100° Medium Stress)]] |
||
− | *[[Media:39-Medium-stress SiNx at 100C using Unaxis ICP deposition tool.pdf|Film Properties of Medium-stress SiN<sub>x</sub> (No Ar, 50W, 100°)]] |
||
− | *[[Media:PECVD2-SiN-Recipe-NoAr-120W-100C-Low-Stress.pdf|SiN Deposition Recipe - No Ar (120W 100° Low Stress)]] |
||
− | *[[Media:37-Low-stress SiNx at 100 C using Unaxis ICP deposition tool.pdf|Film Properties of Low-stress SiN<sub>x</sub> (No Ar, 120W, 100°)]] |
||
− | | |
||
− | *[[Media:PECVD2-SiN-Recipe-NoAr-5W-250C-High-Stress.pdf|SiN Deposition Recipe - No Ar (5W 250° High Stress)]] |
||
− | *[[Media:34-High-stress SiNx at 250 C using Unaxis ICP deposition tool.pdf|Film Properties of High-stress SiN<sub>x</sub> (No Ar, 5W, 250°)]] |
||
− | *[[Media:PECVD2-SiN-Recipe-NoAr-50W-250C-Medium-Stress.pdf|SiN Deposition Recipe - No Ar (50W 250° Medium Stress)]] |
||
− | *[[Media:36-Medium-stress SiNx using Unaxis ICP deposition tool-a.pdf|Film Properties of Medium-stress SiN<sub>x</sub> (No Ar, 50W, 250°)]] |
||
− | *[[Media:PECVD2-SiN-Recipe-NoAr-120W-250C-Low-Stress.pdf|SiN Deposition Recipe - No Ar (120W 250° Low Stress)]] |
||
− | *[[Media:35-Low-stress SiNx at 250 C using Unaxis ICP deposition tool.pdf|Film Properties of Low-stress SiN<sub>x</sub> (No Ar, 120W, 250°)]] |
||
− | |- |
||
− | |} |
||
+ | ==SiO2 HDR 250C Deposition (Unaxis VLR)== |
||
− | === SiN (2% SiH<sub>4</sub> - No-Ar - Extra N<sub>2</sub>) === |
||
+ | ''High-Deposition Rate SiO<sub>2</sub>'' |
||
− | {| class="wikitable" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center;" border="1" |
||
− | |- bgcolor="#D0E7FF" |
||
− | ! width="350" align="center" |50° (pinholes) |
||
− | ! width="350" align="center" |100° (pinholes) |
||
− | ! width="350" align="center" |250° |
||
− | |- align="left" |
||
− | | |
||
− | *[[Media:PECVD2-SiN-Recipe-NoAr-ExtraN2-120W-50C-Low-Stress.pdf|SiN Deposition Recipe - No Ar Extra N<sub>2</sub> (120W 50° Low Stress)]] |
||
− | | |
||
− | *[[Media:PECVD2-SiN-Recipe-NoAr-ExtraN2-120W-100C-Low-Stress.pdf|SiN Deposition Recipe - No Ar Extra N<sub>2</sub> (120W 100° Low Stress)]] |
||
− | | |
||
− | *[[Media:PECVD2-SiN-Recipe-NoAr-ExtraN2-120W-250C-Low-Stress.pdf|SiN Deposition Recipe - No Ar Extra N<sub>2</sub> (120W 250° Low Stress)]] |
||
− | |- |
||
− | |} |
||
+ | ==== Historical Data ==== |
||
− | === SiN (100% SiH<sub>4</sub> ) === |
||
+ | ===== Thin-Film Properties ===== |
||
− | {| class="wikitable" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center;" border="1" |
||
+ | This data is for 180sec long SiO2 HDR ( high deposition rate) deposition, and cleaning time is 900sec, following the procedure [[here]]. |
||
− | |- bgcolor="#D0E7FF" |
||
+ | *[https://docs.google.com/spreadsheets/d/16s-tUna9xrkKneK1lE-qSPuUHWlDmP6Qu3IngBXP3R8/edit#gid=sharing SiO2 HDR 250C 300nm Data-2019] |
||
− | ! width="350" align="center" |50° (pinholes) |
||
+ | *[https://docs.google.com/spreadsheets/d/1OxHi5r9ifNvF8ODpIk6aoRevb4RdbbykwPVMm1g-yi4/edit#gid=sharing SiO2 HDR 250C 300nm Data-2020] |
||
− | ! width="350" align="center" |100° (pinholes) |
||
+ | ===== Uniformity Data ===== |
||
− | ! width="350" align="center" |250° |
||
+ | *[https://docs.google.com/spreadsheets/d/1Mm_rsTm9xDQ50kZx6X6EZ5dTegUvinq0zFxRtE8B2R4/edit#gid=sharing Thickness Uniformity SiO2 HDR 250C 300nm-2019] |
||
− | |- align="left" |
||
+ | *[https://docs.google.com/spreadsheets/d/1nzVeCKsmgL17zft6axQlixpvsEowJOG7qCnLQm_0XxE/edit#gid=sharing Thickness Uniformity SiO2 HDR 250C 300nm-2020] |
||
− | | |
||
− | *[[Media:PECVD2-SiN-Recipe-Low stress SiNx-100%SiH4-120W-50C.pdf|SiN Deposition Recipe (120W 50° Low Stress)]] |
||
− | | |
||
− | *[[Media:PECVD2-SiN-Recipe-Low stres SiNx-100% SiH4-120W-100C.pdf|SiN Deposition Recipe (120W 100° Low Stress)]] |
||
− | *[[Media:PECVD2-SiN-Table-Low stres SiNx-100% SiH4-120W-100C.pdf|SiN Comparison Table 120W-100(250)C]] |
||
− | | |
||
− | *[[Media:PECVD2-SiN-Recipe-Low stress SiNx-100% SiH4-120W-250C.pdf|SiN Deposition Recipe (120W 250° Low Stress)]] |
||
− | *[[Media:PECVD2-SiN-Table-Low stres SiNx-100% SiH4-120W-100C.pdf|SiN Comparison Table 120W, 100(250)C]] |
||
− | |- align="left" |
||
− | | |
||
− | *[[Media:PECVD2-SiN-Recipe-Medium stress SiNx-100%SiH4-120W-50C.pdf|SiN Deposition Recipe (50W 50° Medium Stress)]] |
||
− | | |
||
− | *[[Media:PECVD2-SiN-Recipe-Medium stres SiNx-100% SiH4-120W-100C.pdf|SiN Deposition Recipe (50W 100° Medium Stress)]] |
||
− | *[[Media:PECVD2-SiN-Table-Low stres SiNx-100% SiH4-120W-100C.pdf|SiN Comparison Table 50W, 100(250)C]] |
||
− | *[[Media:27-SiNx_Film_(Bias%3D50W)_Sidewall_Coverage.pdf|SiN SEM sidewall coverage]] |
||
− | | |
||
− | *[[Media:PECVD2-SiN-Recipe-Medium stress SiNx-100% SiH4-120W-250C.pdf|SiN Deposition Recipe (50W 250° Medium Stress)]] |
||
− | *[[Media:PECVD2-SiN-Table-Low stres SiNx-100% SiH4-120W-100C.pdf|SiN ComparisonTable 50W, 100(250)C]] |
||
− | |- |
||
− | |} |
||
− | == |
+ | == SiN 250C deposition (Unaxis VLR) == |
+ | ==== Historical Data ==== |
||
− | === SiO<sub>2</sub> (2% SiH<sub>4</sub>) === |
||
+ | ===== Thin-Film Properties ===== |
||
− | {| class="wikitable" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center;" border="1" |
||
+ | This data is for 480sec long SiN deposition, and cleaning time is 1500sec, following the procedure [[here]]. |
||
− | |- bgcolor="#D0E7FF" |
||
+ | *[https://docs.google.com/spreadsheets/d/1VrgS0cB2OcdZVTCnDAesgQCLRaAgEB_Iajc_OrhXOo0/edit#gid=sharing SiN 250C 300nm Data-2020] |
||
− | ! width="350" align="center" |50° |
||
+ | ===== Uniformity Data ===== |
||
− | ! width="350" align="center" |100° |
||
+ | *[https://docs.google.com/spreadsheets/d/1YAx_Ix84xId8CAhDwZeFT7jLFUwg-BET9aBwg3DxUmQ/edit#gid=sharing Thickness Uniformity SiN 250C 300nm-2020] |
||
− | ! width="350" align="center" |250° |
||
− | |- align="left" |
||
− | | |
||
− | *[[Media:PECVD2-SiO2Recipe-5W-50C.pdf|SiO<sub>2</sub> Deposition Recipe (5W 50°)]] |
||
− | | |
||
− | *[[Media:PECVD2-SiO2Recipe-5W-100C.pdf|SiO<sub>2</sub> Deposition Recipe (5W 100°)]] |
||
− | *[[Media:SiO2 film Unaxis ICP vs PECVD I.pdf|SiO<sub>2</sub> film Unaxis ICP vs PECVD I]] |
||
− | *[[Media:SEM pictures SiO2 100C.pdf|SiO<sub>2</sub> SEM pictures 100C]] |
||
− | | |
||
− | *[[Media:PECVD2-SiO2Recipe-5W-250C.pdf|SiO<sub>2</sub> Deposition Recipe (5W 250°)]] |
||
− | *[[Media:SiO2 film Unaxis ICP vs PECVD I.pdf|SiO<sub>2</sub> film Unaxis ICP vs PECVD I]] |
||
− | |- |
||
− | |} |
||
+ | == SiN LS 250C Deposition (Unaxis VLR) == |
||
− | === SiO<sub>2</sub> (2% SiH<sub>4</sub> - No Ar) === |
||
+ | ''Low Stress Silicon-Nitride'' |
||
− | {| class="wikitable" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center;" border="1" |
||
− | |- bgcolor="#D0E7FF" |
||
− | ! width="350" align="center" |50° |
||
− | ! width="350" align="center" |100° |
||
− | ! width="350" align="center" |250° |
||
− | |- align="left" |
||
− | | |
||
− | *[[Media:PECVD2-SiO2-Recipe-NoAr-50C.pdf|SiO<sub>2</sub> Deposition Recipe - No Ar (50°)]] |
||
− | *[[Media:29-UnaxisPM3-SiO2-SiH4-O2-He.pdf|SiO<sub>2</sub> Film Properties-No Ar]] |
||
− | | |
||
− | *[[Media:PECVD2-SiO2-Recipe-NoAr-100C.pdf|SiO<sub>2</sub> Deposition Recipe - No Ar (100°)]] |
||
− | *[[Media:29-UnaxisPM3-SiO2-SiH4-O2-He.pdf|SiO<sub>2</sub> Film Properties-No Ar]] |
||
− | | |
||
− | *[[Media:PECVD2-SiO2-Recipe-NoAr-250C.pdf|SiO<sub>2</sub> Deposition Recipe - No Ar (250°)]] |
||
− | *[[Media:29-UnaxisPM3-SiO2-SiH4-O2-He.pdf|SiO<sub>2</sub> Film Properties-No Ar]] |
||
− | |- |
||
− | |} |
||
+ | ==== Historical Data ==== |
||
− | === SiO<sub>2</sub> (100% SiH<sub>4</sub> HDR) === |
||
+ | ''To Be Added'' |
||
− | {| class="wikitable" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center;" border="1" |
||
− | |- bgcolor="#D0E7FF" |
||
− | ! width="350" align="center" |50° |
||
− | ! width="350" align="center" |100° |
||
− | ! width="350" align="center" |250° |
||
− | |- align="left" |
||
− | | |
||
− | *[[Media:SiO2 100% SiH4 HDR 50C.pdf|SiO<sub>2</sub> Deposition Recipe - HDR (50°)]] |
||
− | | |
||
− | *[[Media:PECVD2-SiO2-Recipe-100%SiH4-HDR-100C.pdf|SiO<sub>2</sub> Deposition Recipe - HDR (100°)]] |
||
− | *[[Media:PECVD2-SiO2-HDR-100% SiH4.pdf|SiO<sub>2</sub> Comparison Table - HDR (100°)]] |
||
− | | |
||
− | *[[Media:PECVD2-SiO2-Recipe-100%SiH4-HDR-250C.pdf|SiO<sub>2</sub> Deposition Recipe - HDR (250°)]] |
||
− | *[[Media:PECVD2-SiO2-HDR-100% SiH4.pdf|SiO<sub>2</sub> Comparison Table - HDR (250°)]] |
||
− | |- |
||
− | |} |
||
+ | ===== Thin-Film Properties ===== |
||
− | === SiO<sub>2</sub> (100% SiH<sub>4</sub> LDR) === |
||
+ | This data is for 180sec long SiN LS (low stress) deposition, and cleaning time is 1500sec, following the procedure [[here]]. |
||
− | {| class="wikitable" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center;" border="1" |
||
+ | *[https://docs.google.com/spreadsheets/d/1i2mE2K12EEulnCbO9KuU9PCcvHAmcGxTIXUF8x4IOWk/edit#gid=sharing SiN LS 250C 300nm Data-2020] |
||
− | |- bgcolor="#D0E7FF" |
||
+ | ===== Uniformity Data ===== |
||
− | ! width="350" align="center" |50° |
||
+ | *[https://docs.google.com/spreadsheets/d/1NDyxH1i9COM2XTryLqYPE9yOekgRslAJUO7o56iTOEQ/edit#gid=sharing Thickness Uniformity SiN LS 250C 300nm-2020] |
||
− | ! width="350" align="center" |100° |
||
− | ! width="350" align="center" |250° |
||
− | |- align="left" |
||
− | | |
||
− | *[[Media:PECVD2-SiO2-Recipe-100%SiH4-LDR-50C.pdf|SiO<sub>2</sub> Deposition Recipe - LDR (50°)]] |
||
− | | |
||
− | *[[Media:PECVD2-SiO2-Recipe-100%SiH4-LDR-100C.pdf|SiO<sub>2</sub> Deposition Recipe - LDR (100°)]] |
||
− | *[[Media:PECVD2-SiO2-LDR-100% SiH4.pdf|SiO<sub>2</sub> Comparison Table - LDR (100°)]] |
||
− | *[[Media:PECVD2-SiO2-SEM-LDR SiO2-100% SiH4-100C-15W.pdf|SiO<sub>2</sub> SEM sidewall coverage]] |
||
− | | |
||
− | *[[Media:PECVD2-SiO2-Recipe-100%SiH4-LDR-250C.pdf|SiO<sub>2</sub> Deposition Recipe - LDR (250°)]] |
||
− | *[[Media:PECVD2-SiO2-LDR-100% SiH4.pdf|SiO<sub>2</sub> Comparison Table - LDR (250°)]] |
||
− | |- |
||
− | |} |
||
− | + | == Cleaning Recipes (Unaxis VLR Dep) == |
|
+ | You must edit the Post-Dep Clean recipe to correspond to your deposited thickness and material. See the [[ICP-PECVD (Unaxis VLR)#Documentation|Operating Procedure on the Unaxis Tool Page]] for details. |
||
− | {| class="wikitable" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center;" border="1" |
||
+ | * SiNx etches at 20nm/min |
||
− | |- bgcolor="#D0E7FF" |
||
+ | * SiO2 etches at 40nm/min |
||
− | ! width="350" align="center" |90° |
||
− | ! width="350" align="center" |250° |
||
− | |- align="left" |
||
− | | |
||
− | *[[Media:02-ICP-PECVD-a-Si Film-90C.pdf|a-Si Deposition Recipe - 90°]] |
||
− | | |
||
− | *[[Media:01-ICP-PECVD-a-Si-Deposition Recipe-250C.pdf|a-Si Deposition Recipe - 250°]] |
||
− | *[[Media:Amorphous Silicon Film Deposition using 12.5W bias on SiO2-Si.pdf|Thick, Defects-free a-Si Film on SiO<sub>2</sub>/Si with a Lower Bias Power]] |
||
− | |- |
||
− | |} |
Revision as of 15:47, 19 February 2021
Back to Vacuum Deposition Recipes.
PECVD 1 (PlasmaTherm 790)
Historical Particulate Data
- Particulates(Gain4) in PECVD#1-OLD DATA 2015
- Particulates(Gain4) in PECVD#1-OLD DATA 2016
- Particulates(Gain4) in PECVD#1-OLD DATA 2017
- Particulates in PECVD#1 films 2017
- Particulates in PECVD#1 films 2018
- Particulates in PECVD#1 films 2019
- Particulates in PECVD#1 films 2020
- Particulates in PECVD#1 films 2021
SiN deposition (PECVD #1)
Historical Data
Thin-Film Properties
- SiN 100nm Data 2014
- SiN 100nm Data 2015
- SiN 100nm Data 2016
- SiN 100nm Data 2017
- SiN 300nm Data 2017
- SiN 300nm Data 2018
- SiN 300nm Data 2019
- SiN 300nm Data 2020
- SiN 300nm Data 2021
Uniformity Data
- SiN 100 nm Thickness uniformity 2014
- SiN 100 nm Thickness uniformity 2015
- SiN 100 nm Thickness uniformity 2016
- SiN 100 nm Thickness uniformity 2017
- SiN 300nm Thickness uniformity 2017
- SiN 300nm Thickness uniformity 2018
- SiN 300nm Thickness uniformity 2019
- SiN 300nm Thickness uniformity 2020
- SiN 300nm Thickness uniformity 2021
SiO2 deposition (PECVD #1)
Historical Data
Thin-Film Properties
- SiO2 100nm Data 2014
- SiO2 100nm Data 2015
- SiO2 100nm Data 2016
- SiO2 100nm Data 2017
- SiO2 300nm Data 2017
- SiO2 300nm Data 2018
- SiO2 300nm Data 2019
- SiO2 300nm Data 2020
- SiO2 300nm Data 2021
Thick-Film Properties
Uniformity Data
- SiO2 100nm Thickness uniformity 2014
- SiO2 100 nm Thickness uniformity 2015
- SiO2 100 nmThickness uniformity 2016
- SiO2 100nm Thickness uniformity 2017
- SiO2 300nm Thickness uniformity 2017
- SiO2 300nm Thickness uniformity 2018
- SiO2 300nm Thickness uniformity 2019
- SiO2 300nm Thickness uniformity 2020
- SiO2 300nm Thickness uniformity 2021
Low-Stress SiN - LS-SiN (PECVD#1)
SiOxNy deposition (PECVD #1)
Cleaning Recipes (PECVD #1)
The cleaning procedure is very important in order to have consistent result on this tool and also to keep particulate count low. After each deposition you should clean the tool following instructions carefully. The clean is done in two steps:
- Wet cleaning (start cleaning by using a cleanroom wipe sprayed with DI. Wipe chamber sidewalls with it. Finish cleaning by using the cleanroom wipe sprayed with IPA. )
- Load the recipe for cleaning "CF4/O2 Clean" (edit the recipe and change ONLY time of cleaning). Follow instructions regarding a required time for cleaning.
Standard Cleaning Recipe: "CF4/O2 Clean"
Click the above link for a screenshot of the standard cleaning recipe, for which you will enter a custom time. The recipe is set up so that it will pop up a window for the cleaning time upon running the recipe - you do not need to edit the recipe before running it.
PECVD 2 (Advanced Vacuum)
Historical Particulate Data
- Particulates (Gain4) in PECVD#2 2015
- Particulates (Gain4) in PECVD#2 2016
- Particulates (Gain4) in PECVD#2 2017
- Particulates in PECVD#2 films 2017
- Particulates in PECVD#2 films 2018
- Particulates in PECVD#2 films 2019
- Particulates in PECVD#2 films 2020
- Particulates in PECVD#2 films 2021
SiO2 deposition (PECVD #2)
Standard Recipe
Historical Data
Thin-Film Properties
- Oxide Data 2014
- Oxide Data 2015
- Oxide data 2016
- Oxide Data 2017
- Oxide Data 2018
- Oxide Data 2019
- Oxide Data 2020
- Oxide Data 2021
Thin-Film Properties
Uniformity Data
- Oxide Thickness Uniformity 2014
- Oxide Thickness Uniformity 2015
- Oxide Thickness Uniformity 2016
- Oxide Thickness Uniformity 2017
- Oxide Thickness Uniformity 2018
- Oxide Thickness Uniformity 2019
- Oxide Thickness Uniformity 2020
- Oxide Thickness Uniformity 2021
SiN deposition (PECVD #2)
Standard Recipe
Historical Data
Thin-Film Properties
- Nitride2 Data 2014
- Nitride2 Data 2015
- Nitride2 Data 2016
- Nitride2 Data 2017
- Nitride2 Data 2018
- Nitride2 Data 2019
- Nitride2 Data 2020
- Nitride2 Data 2021
Uniformity Data
- Nitride2 Thickness Uniformity 2014
- Nitride2 Thickness Uniformity 2015
- Nitride2 Thickness Uniformity 2016
- Nitride2 Thickness Uniformity 2017
- Nitride2 Thickness Uniformity 2018
- Nitride2 Thickness Uniformity 2019
- Nitride2 Thickness Uniformity 2020
- Nitride2 Thickness Uniformity 2021
Low-Stress SiN deposition (PECVD #2)
Low-Stress SilIcon Nitride (< 100 MPa)
Standard Recipe
- STD LS Nitride2 Recipe
- Old Versions:
Historical Data
Thin-Film Properties
- LS Nitride2 Data 2014
- LS Nitride2 Data 2015
- LS Nitride2 Data 2016
- LS Nitride2 Data 2017
- LS Nitride2 Data 2018
- LS Nitride2 Data 2019
- LS Nitride2 Data 2020
- LS Nitride2 Data 2021
Uniformity Data
- LS Nitride2 Thickness Uniformity 2014
- LS Nitride2 Thickness Uniformity 2015
- LS Nitride2 Thickness Uniformity 2016
- LS Nitride2 Thickness Uniformity 2017
- LS Nitride2 Thickness Uniformity 2018
- LS Nitride2 Thickness Uniformity 2019
- LS Nitride2 Thickness Uniformity 2020
- LS Nitride2 Thickness Uniformity 2021
Amorphous-Si deposition (PECVD #2)
Cleaning Recipes (PECVD #2)
The cleaning procedure is very important in order to have consistent result on this tool and also to keep particulate count low. After each deposition you should clean the tool following instructions carefully. The clean is done in two steps:
- Wet cleaning (start cleaning by using a cleanroom wipe sprayed with DI. Wipe chamber sidewalls with it. Finish cleaning by using the cleanroom wipe sprayed with IPA. )
- Load the recipe for cleaning "STD CF4/O2 Clean" (edit the recipe and change ONLY time of cleaning). Follow instructions regarding a required time for cleaning.
Standard Clean Recipe: "STD CF4/O2 Clean recipe"
Click the above link for a screenshot of the standard cleaning recipe, for which you will enter a custom time. The recipe is set up so that it will pop up a window for the cleaning time upon running the recipe - you do not need to edit the recipe before running it.
ICP-PECVD (Unaxis VLR)
2020-02: New recipes have been characterized for low particulate count and repeatability. Only staff-supplied recipes are allowed in the tool. Please follow the new procedures to ensure low particle counts in the chamber.
The system currently has Deuterated Silane (SiD4) installed - identical to the regular Silicon precursor SiH4, except that it significantly lowers optical absorption in the near-infrared due to shifted molecular vibrations/molecular weights.
Historical Particulate Data
Standard Recipes
SiO2 LDR 250C Deposition (Unaxis VLR)
Low-Deposition Rate SiO2
Historical Data
Thin-Film Properties
This data is for 780sec long SiO2 LDR (low deposition rate) deposition, and cleaning time is 900sec, following the procedure here.
Uniformity Data
SiO2 HDR 250C Deposition (Unaxis VLR)
High-Deposition Rate SiO2
Historical Data
Thin-Film Properties
This data is for 180sec long SiO2 HDR ( high deposition rate) deposition, and cleaning time is 900sec, following the procedure here.
Uniformity Data
SiN 250C deposition (Unaxis VLR)
Historical Data
Thin-Film Properties
This data is for 480sec long SiN deposition, and cleaning time is 1500sec, following the procedure here.
Uniformity Data
SiN LS 250C Deposition (Unaxis VLR)
Low Stress Silicon-Nitride
Historical Data
To Be Added
Thin-Film Properties
This data is for 180sec long SiN LS (low stress) deposition, and cleaning time is 1500sec, following the procedure here.
Uniformity Data
Cleaning Recipes (Unaxis VLR Dep)
You must edit the Post-Dep Clean recipe to correspond to your deposited thickness and material. See the Operating Procedure on the Unaxis Tool Page for details.
- SiNx etches at 20nm/min
- SiO2 etches at 40nm/min