Difference between revisions of "PECVD1 Recipes"

From UCSB Nanofab Wiki
Jump to navigation Jump to search
Line 38: Line 38:
 
== LS SiN deposition (PECVD #1) ==
 
== LS SiN deposition (PECVD #1) ==
 
<!-- Placeholders - Not uploaded yet-->
 
<!-- Placeholders - Not uploaded yet-->
*[[media:PECVD1-SiN-Recipe.pdf|LS SiN Deposition Recipes - Varying N/O Ratio]]
+
*[[media:LS SiN Deposition Recipes - Varying N/O Ratio]]
 
*[[media:PECVD1-SiN-Plot.pdf|LS SiN Stress/Index vs. O/N Ratio]]
 
*[[media:PECVD1-SiN-Plot.pdf|LS SiN Stress/Index vs. O/N Ratio]]
 
*[[media:PECVD1-LS SIN recipe 2014.pdf|LS SiN Recipe]]
 
*[[media:PECVD1-LS SIN recipe 2014.pdf|LS SiN Recipe]]

Revision as of 16:36, 5 December 2014

PECVD 1 (PlasmaTherm 790)

SiN deposition (PECVD #1)

  • Deposition rate~11.23nm/min (users must calibrate this prior to critical deps)
  • HF e.r.~89nm/min
  • Stress~450MPa
  • Refractive Index~1.942

SiO2 deposition (PECVD #1)

  • Deposition rate~35.52nm/min (users must calibrate this prior to critical deps)
  • HF e.r.~645nm/min
  • Stress~-408MPa
  • Refractive Index~1.461

SiOxNy deposition (PECVD #1)

  • Deposition rate~14.99nm/min (users must calibrate this prior to critical deps)
  • HF e.r.~417nm/min
  • Stress~133MPa
  • Refractive Index~1.714

LS SiN deposition (PECVD #1)

  • Deposition rate~14.99nm/min (users must calibrate this prior to critical deps)
  • HF e.r.~417nm/min
  • Stress~133MPa