== SiN deposition (PECVD #1) == |
== SiN deposition (PECVD #1) == |
||
*[[media:PECVD1-SiN-standard recipe 2014.pdf|SiN Standard Recipe]] |
*[[media:PECVD1-SiN-standard recipe 2014.pdf|SiN Standard Recipe]] |
||
− | *[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dEN6LV93LXlnbUhIWU1adVZWMWlXYnc&usp=drive_web#gid=sharing SiN Data |
+ | *[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dEN6LV93LXlnbUhIWU1adVZWMWlXYnc&usp=drive_web#gid=sharing SiN Data November 2014] |
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dElmTXZyOEZsOFdrMVhNLWpKXzVmNWc&usp=sharing SiN 1000A Thickness uniformity 2014] |
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dElmTXZyOEZsOFdrMVhNLWpKXzVmNWc&usp=sharing SiN 1000A Thickness uniformity 2014] |
||
<!-- Placeholders - Not uploaded yet--> |
<!-- Placeholders - Not uploaded yet--> |
Revision as of 10:01, 2 December 2014
PECVD 1 (PlasmaTherm 790)
SiN deposition (PECVD #1)
- SiN Standard Recipe
- SiN Data November 2014
- SiN 1000A Thickness uniformity 2014
- Low Stress Si3N4 - Variable Stress Recipes
- Low Stress Si3N4 - Variable Stress Plot
- Deposition rate~11.25nm/min (users must calibrate this prior to critical deps)
- HF e.r.~89nm/min
- Stress~446MPa
- Refractive Index~1.940
SiO2 deposition (PECVD #1)
- HF e.r.~639nm/min
- Stress~-415MPa
- Refractive Index~1.461
SiOxNy deposition (PECVD #1)
- SiOxNy Deposition Recipes - Varying N/O Ratio
- SiOxNy Stress/Index vs. O/N Ratio
- SiOxNy Recipe
- SiOxNy Data October 2014
- SiOxNy 3000A Thickness uniformity 2014
- Deposition rate~14.65nm/min (users must calibrate this prior to critical deps)
- HF e.r.~411nm/min
- Stress~137MPa
- Refractive Index~1.712