Difference between revisions of "PECVD1 Recipes"
Jump to navigation
Jump to search
Line 27: | Line 27: | ||
*[[media:PECVD1-SiON-Recipe.pdf|SiO<sub>x</sub>N<sub>y</sub> Deposition Recipes - Varying N/O Ratio]] |
*[[media:PECVD1-SiON-Recipe.pdf|SiO<sub>x</sub>N<sub>y</sub> Deposition Recipes - Varying N/O Ratio]] |
||
*[[media:PECVD1-SiON-Plot.pdf|SiO<sub>x</sub>N<sub>y</sub> Stress/Index vs. O/N Ratio]] |
*[[media:PECVD1-SiON-Plot.pdf|SiO<sub>x</sub>N<sub>y</sub> Stress/Index vs. O/N Ratio]] |
||
+ | |||
+ | |||
+ | == SiO<sub>2</sub> deposition (PECVD #1) == |
||
+ | *[[media:PECVD1-SiO2-standard recipe 2014.pdf|SiO<sub>2</sub> Standard Recipe]] |
||
+ | *[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dEw0bjFEdTF2SUhRa25Ca0d0SzBha3c&usp=drive_web#gid=sharing SiO<sub>2</sub> Data September 2014] |
||
+ | *[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dEttR2JSTkRoamR0SUZ4bE5QUW9uS2c&usp=sharing SiO<sub>2</sub> 1000A Thickness uniformity 2014] |
||
+ | |||
+ | *Deposition rate~35.22nm/min (users must calibrate this prior to critical deps) |
||
+ | *HF e.r.~646nm/min |
||
+ | *Stress~-407MPa |
||
+ | *Refractive Index~1.460 |
Revision as of 11:27, 16 September 2014
PECVD 1 (PlasmaTherm 790)
SiN deposition (PECVD #1)
- SiN Standard Recipe
- SiN Data September 2014
- SiN 1000A Thickness uniformity 2014
- Low Stress Si3N4 - Variable Stress Recipes
- Low Stress Si3N4 - Variable Stress Plot
- Deposition rate~11.30nm/min (users must calibrate this prior to critical deps)
- HF e.r.~90nm/min
- Stress~444MPa
- Refractive Index~1.940
SiO2 deposition (PECVD #1)
- Deposition rate~35.22nm/min (users must calibrate this prior to critical deps)
- HF e.r.~646nm/min
- Stress~-407MPa
- Refractive Index~1.460
SiOxNy deposition (PECVD #1)
SiO2 deposition (PECVD #1)
- Deposition rate~35.22nm/min (users must calibrate this prior to critical deps)
- HF e.r.~646nm/min
- Stress~-407MPa
- Refractive Index~1.460