OLD - PECVD2 Recipes
Revision as of 15:13, 24 September 2014 by Biljana (talk | contribs) (→LS SiN deposition (PECVD #2))
PECVD 2 (Advanced Vacuum)
SiN deposition (PECVD #2)
- Deposition Rate: ≈ 8.17 nm/min (users must calibrate this prior to critical deps)
- Refractive Index: ≈ 1.957
- Stress ≈ 499MPa
- HF etch rate:~49nm/min
SiO2 deposition (PECVD #2)
- Deposition Rate: ≈ 28.50 nm/min (users must calibrate this prior to critical deps)
- Refractive Index: ≈ 1.474
- Stress ≈ -252MPa
- HF etch rate~616nm/min
LS SiN deposition (PECVD #2)
- Deposition Rate: ≈ 8.14 nm/min (users must calibrate this prior to critical deps)
- Refractive Index: ≈ 1.935
- Stress ≈ -7.18MPa
- HF etch rate~48nm/min