Difference between revisions of "OLD - PECVD2 Recipes"

From UCSB Nanofab Wiki
Jump to navigation Jump to search
Line 23: Line 23:
   
 
*[[media:AdvPECVD-LS Nitride2 300C standard recipe.pdf|LS Nitride2 Standard Recipe]]
 
*[[media:AdvPECVD-LS Nitride2 300C standard recipe.pdf|LS Nitride2 Standard Recipe]]
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dEZvWVhzS1pHUXZkOGcyQWZ4LTNBWGc&usp=drive_web#gid=sharing LS Nitride2 Data May 2014]
+
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dEZvWVhzS1pHUXZkOGcyQWZ4LTNBWGc&usp=drive_web#gid=sharing LS Nitride2 Data June 2014]
   
 
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dENSak1ZNnVaVTFEQTBzdDJMSDlDTFE&usp=drive_web#gid=1=sharing LS Nitride2 Thickness uniformity 2014]
 
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dENSak1ZNnVaVTFEQTBzdDJMSDlDTFE&usp=drive_web#gid=1=sharing LS Nitride2 Thickness uniformity 2014]

Revision as of 15:24, 11 June 2014

PECVD 2 (Advanced Vacuum)

SiN deposition (PECVD #2)

  • Deposition Rate: ≈ 8.29 nm/min (users must calibrate this prior to critical deps)
  • Refractive Index: ≈ 1.955
  • Stress ≈ 498MPa
  • HF etch rate:~48nm/min

SiO2 deposition (PECVD #2)

  • Deposition Rate: ≈ 28.36 nm/min (users must calibrate this prior to critical deps)
  • Refractive Index: ≈ 1.473
  • Stress ≈ -256MPa
  • HF etch rate~582nm/min

LS SiN deposition (PECVD #2)

  • Deposition Rate: ≈ 8.17 nm/min (users must calibrate this prior to critical deps)
  • Refractive Index: ≈ 1.935
  • Stress ≈ -0.04MPa
  • HF etch rate~47nm/min

Amorphous-Si deposition (PECVD #2)