Difference between revisions of "OLD - PECVD2 Recipes"
Jump to navigation
Jump to search
m (John d moved page PECVD2 Recipes to OLD - PECVD2 Recipes without leaving a redirect: this page is not linked anywhere, looks like 2014 data only) |
|||
(12 intermediate revisions by one other user not shown) | |||
Line 3: | Line 3: | ||
==Photos== |
==Photos== |
||
− | *[[media: |
+ | *[[media: Photos Sheet1.pdf|Dirty platen]] |
− | |||
⚫ | |||
⚫ | |||
⚫ | |||
⚫ | |||
− | |||
− | *Deposition Rate: ≈ 7.93 nm/min (users must calibrate this prior to critical deps) |
||
− | *Refractive Index: ≈ 1.961 |
||
− | *Stress ≈ 495MPa |
||
− | *HF etch rate:~49nm/min |
||
== SiO<sub>2</sub> deposition (PECVD #2) == |
== SiO<sub>2</sub> deposition (PECVD #2) == |
||
− | *[[media: |
+ | *[[media:NewAdvPECVD OXIDE 300C standard recipe.pdf|Oxide Standard Recipe]] |
− | *[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dGJZaGtDTVRqa1BRdW5iU1N1Y01jd0E&usp=drive_web#gid=sharing Oxide Data |
+ | *[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dGJZaGtDTVRqa1BRdW5iU1N1Y01jd0E&usp=drive_web#gid=sharing Oxide Data 2014] |
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dDRjSHEtYUZRUTg4azE2U0JGUTg2M1E#gid=sharing Oxide Thickness uniformity 2014] |
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dDRjSHEtYUZRUTg4azE2U0JGUTg2M1E#gid=sharing Oxide Thickness uniformity 2014] |
||
⚫ | |||
− | *Deposition Rate: ≈ 28.64 nm/min (users must calibrate this prior to critical deps) |
||
⚫ | |||
− | *Refractive Index: ≈ 1.475 |
||
⚫ | |||
− | *Stress ≈ -260MPa |
||
⚫ | |||
− | *HF etch rate~623nm/min |
||
==LS SiN deposition (PECVD #2) == |
==LS SiN deposition (PECVD #2) == |
||
⚫ | |||
− | |||
⚫ | |||
⚫ | |||
⚫ | |||
− | |||
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dENSak1ZNnVaVTFEQTBzdDJMSDlDTFE&usp=drive_web#gid=1=sharing LS Nitride2 Thickness uniformity 2014] |
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dENSak1ZNnVaVTFEQTBzdDJMSDlDTFE&usp=drive_web#gid=1=sharing LS Nitride2 Thickness uniformity 2014] |
||
− | |||
− | *Deposition Rate: ≈ 7.96 nm/min (users must calibrate this prior to critical deps) |
||
− | *Refractive Index: ≈ 1.937 |
||
− | *Stress ≈ 2.77MPa |
||
− | *HF etch rate~47nm/min |
||
== Amorphous-Si deposition (PECVD #2) == |
== Amorphous-Si deposition (PECVD #2) == |