Difference between revisions of "OLD - PECVD2 Recipes"
Jump to navigation
Jump to search
(Created page with "=PECVD 2 (Advanced Vacuum)= == SiN deposition (PECVD #2) == *Nitride2 Standard Recipe *[[media:ADV PECVD NI...") |
m (John d moved page PECVD2 Recipes to OLD - PECVD2 Recipes without leaving a redirect: this page is not linked anywhere, looks like 2014 data only) |
||
(54 intermediate revisions by one other user not shown) | |||
Line 1: | Line 1: | ||
=[[PECVD 2 (Advanced Vacuum)]]= |
=[[PECVD 2 (Advanced Vacuum)]]= |
||
⚫ | |||
⚫ | |||
− | *[[media:ADV PECVD NITRIDE2-Data April 2014.pdf|Nitride2 Data (Deposition Rate, Refractive Index, Stress, HF etch rate)]] |
||
⚫ | |||
⚫ | |||
+ | ==Photos== |
||
− | *Deposition Rate: ≈ 9.0 nm/min |
||
+ | |||
− | *Refractive Index: ≈ 1.952 |
||
+ | *[[media: Photos Sheet1.pdf|Dirty platen]] |
||
− | *Stress ≈ 484MPa |
||
== SiO<sub>2</sub> deposition (PECVD #2) == |
== SiO<sub>2</sub> deposition (PECVD #2) == |
||
− | *[[media: |
+ | *[[media:NewAdvPECVD OXIDE 300C standard recipe.pdf|Oxide Standard Recipe]] |
⚫ | |||
− | *[[media:ADV OXIDE data April 2014.pdf|Oxide Data (Deposition Rate, Refractive Index, Stress, HF etch rate )]] |
||
⚫ | |||
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dDRjSHEtYUZRUTg4azE2U0JGUTg2M1E#gid=sharing Oxide Thickness uniformity 2014] |
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dDRjSHEtYUZRUTg4azE2U0JGUTg2M1E#gid=sharing Oxide Thickness uniformity 2014] |
||
⚫ | |||
− | *Deposition Rate: ≈ 28.0 nm/min |
||
⚫ | |||
− | *Refractive Index: ≈ 1.472 |
||
⚫ | |||
− | *Stress ≈ -270MPa |
||
⚫ | |||
==LS SiN deposition (PECVD #2) == |
==LS SiN deposition (PECVD #2) == |
||
⚫ | |||
− | |||
⚫ | |||
⚫ | |||
− | *[[media:New Advanced PECVD LS NITRIDE2 April 2014.pdf|LS Nitride2 Data (Deposition Rate, Refractive Index, Stress, HF etch rate )]] |
||
⚫ | |||
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dENSak1ZNnVaVTFEQTBzdDJMSDlDTFE&usp=drive_web#gid=1=sharing LS Nitride2 Thickness uniformity 2014] |
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dENSak1ZNnVaVTFEQTBzdDJMSDlDTFE&usp=drive_web#gid=1=sharing LS Nitride2 Thickness uniformity 2014] |
||
− | |||
− | *Deposition Rate: ≈ 8.34 nm/min |
||
− | *Refractive Index: ≈ 1.932 |
||
− | *Stress ≈ -45MPa |
||