How to measure thin ≤50nm metal dep. rates using ellipsometry. Also useful for Witness samples (ie. inserted for deposition along with production wafers)
Deposition rate test w/ TOX Witness samples | For thin metals - eg. ≤50nm (exact limit is different for various metals, based on optical absorption) |
Wafers for rate cal: | Silicon with ~500nm-1000nm Thermal Oxide (TOX). Cleave into quarters (2" wafers preferred for easy cleaving). |
Ellipsometer: pre-measure before dep | Normal "Cauchy on Silicon" recipe
Fit only 300nm+ |
Once fit is very good,
[Save Snapshot] somewhere (top-right of window) | |
Metal Deposition: Any technique | |
(optional) Include above TOX Witness piece with sample | |
Target ~10-30nm of dep | If very short (eg. 30sec), make sure uniformity will be ok (eg. AJA substrate rotation is at Max) |
Ellipsometer: measure after dep | |
Measure with "Standard" setting
[√] SAVE DATA |
You can also save data *after* the scan with
Data (top-left of screen) > [Save] Later, we will load this NEW (post-dep) data into the pre-dep Snapshot |
Open Snapshot from pre-measurement | |
Turn off ALL fitting params in Cauchy (thickness, A/B/C)
Turn off Angle fit and set Angle = 0 |
|
Turn off "Fit Options" > "Thickness pre-fit" (I think it's in Model params) | |
Load *new* data with
Data (top-left of screen) > [Open] |
Will still show model + fit from pre-meas. |
Select wavelengths 300nm+ | |
Add Layer Basic > B-SPLINE on top of layer stack | Best fit wih BSPLINE model on top of Cauchy, |
B-Spline params:
- Starting mat = Au - Thickness = 15nm Only fitting Thickness on this layer |
Pre meausred undep'd TOX and then added bspline (with Au starting mat) on top. |
Click Model > [FIT] | Can do [Generate] first to see how close it is. |
[Save Snapshot] when have good fit | |
Record Thickness of B-SPLINE, nm |
Demis D. John, 2022-10-27 - based on J.A.Woollam instructions.