Direct-Write Lithography Recipes
The printable version is no longer supported and may have rendering errors. Please update your browser bookmarks and please use the default browser print function instead.
Work In Progress This article is still under construction. It may contain factual errors. Content is subject to change. |
Maskless Aligner (Heidelberg MLA150)
Photolithography Recipes for the Heidelberg MLA150. Description of litho params- different lasers available, greyscale etc.
Positive Resist (MLA150)
General notes: Hotplates used, filters, laser wavelengths, etc.
Resist | Spin Cond. | Bake | Thickness | Laser (nm) | Exposure Time| | DeFocus | PEB | Developer | Developer Time | Comments |
---|---|---|---|---|---|---|---|---|---|---|
AZ4110 | 4 krpm/30s | 95°C/60s | ~ 1.1 µm | 405 | 240 | 5 | none | AZ400K:DI 1:4 | 50s | Used MLA design (good for isolated lines 0.8-1um) |
AZ4330 | 4 krpm/30s | 95°C/60s | ~ 3.3 µm | 405 | 320 | 6 | none | AZ400K:DI 1:4 | 90s | Used MLA design |
AZ4620 | ||||||||||
SPR 220-3.0 | 2.5 krpm/30s | 115°C/90” | ~ 2.7 µm | 405 | 325 | - 4 | 115°C/90s | AZ300MIF | 60s | Used MLA design |
SPR 955-CM0.9 | 3 krpm/30s | 95°C/90” | ~ 0.9 µm | 405 | 250 | - 7 | 110°C/90s | AZ300MIF | 60s | Used MLA design |
THMR-3600HP |
Negative Resist (MLA150)
General notes: Hotplates used, filters, laser wavelengths, etc.
Resist | Spin Cond. | Bake | Thickness | Laser (nm) | Exposure Time | DeFocus | PEB | Flood | Developer | Developer Time | Comments |
---|---|---|---|---|---|---|---|---|---|---|---|
AZ5214 | 6 krpm/30s | 95°C/60s | ~ 1.0 µm | 375 | 60" | AZ300MIF | 60s |
| |||
AZnLOF2020 | 4 krpm/30s | 110°C/60s | ~ 2.1µm | 375 | 340 | - 3 | none | AZ300MIF | 90s | ||
SU-8 2075 | ~70µm | 375 | Extremely viscous. Pour into a wide-mouthed bottle, dispense directly from bottle. Replace napkin at end. |
Greyscale Lithography (MLA150)
Description...
Resist | Spin Cond. | Bake | Thickness | Exposure Time | Focus Offset | PEB | Flood | Developer | Developer Time | Comments |
---|---|---|---|---|---|---|---|---|---|---|
AZ4620Z5214 | ?? krpm/30” | 95°C/60” | ?? µm | 60" | AZ300MIF | 60" |
|