Line 121: Line 121:
 
|~ 1.0 µm
 
|~ 1.0 µm
 
|375
 
|375
|
+
|35
|
+
| - 5
|
+
|Used UCSB design. Good for up to ~1.3um open line space.
 
|60"
 
|60"
 
|AZ300MIF
 
|AZ300MIF
Line 141: Line 141:
 
|AZ300MIF
 
|AZ300MIF
 
|90s
 
|90s
|Used UCSB design. Good for 2um feature size.  
+
|Used UCSB design. Good for 2um open line space.
 
|-
 
|-
 
|[[:File:SU-8-2075-revA.pdf|SU-8 2075]]
 
|[[:File:SU-8-2075-revA.pdf|SU-8 2075]]

Revision as of 16:37, 9 October 2020

UnderConstruction.jpg

Work In Progress

This article is still under construction. It may contain factual errors. Content is subject to change.


Maskless Aligner (Heidelberg MLA150)

Photolithography Recipes for the Heidelberg MLA150. Description of litho params- different lasers available, greyscale etc.

Positive Resist (MLA150)

General notes: Hotplates used, filters, laser wavelengths, etc.

Resist Spin Cond. Bake Thickness Laser (nm) Exposure Time| DeFocus PEB Developer Developer Time Comments
AZ4110 4 krpm/30s 95°C/60s ~ 1.1 µm 405 240 5 none AZ400K:DI 1:4 50s Used MLA design (good for isolated lines 0.8-1um)
AZ4330 4 krpm/30s 95°C/60s ~ 3.3 µm 405 320 6 none AZ400K:DI 1:4 90s Used MLA design
AZ4620
SPR 220-3.0 2.5 krpm/30s 115°C/90” ~ 2.7 µm 405 325 - 4 115°C/90s AZ300MIF 60s Used MLA design
SPR 955-CM0.9 3 krpm/30s 95°C/90” ~ 0.9 µm 405 250 - 7 110°C/90s AZ300MIF 60s Used MLA design
THMR-3600HP

Negative Resist (MLA150)

General notes: Hotplates used, filters, laser wavelengths, etc.

Resist Spin Cond. Bake Thickness Laser (nm) Exposure Time DeFocus PEB Flood Developer Developer Time Comments
AZ5214 6 krpm/30s 95°C/60s ~ 1.0 µm 375 35 - 5 Used UCSB design. Good for up to ~1.3um open line space. 60" AZ300MIF 60s
  • ???
AZnLOF2020 4 krpm/30s 110°C/60s ~ 2.1µm 375 340 - 3 110°C/60s none AZ300MIF 90s Used UCSB design. Good for 2um open line space.
SU-8 2075 ~70µm 375 Extremely viscous. Pour into a wide-mouthed bottle, dispense directly from bottle. Replace napkin at end.

Greyscale Lithography (MLA150)

Description...

Resist Spin Cond. Bake Thickness Exposure Time Focus Offset PEB Flood Developer Developer Time Comments
AZ4620Z5214 ?? krpm/30” 95°C/60” ?? µm 60" AZ300MIF 60"
  • ???