Conditions

All wafers were spun at 1.5krpm and baked for 60s at various temperatures (200C, 210C, 220C). 

Checked thickness on the ellipsometer, developed in 300MIF for 30s and check thickness again.

Develop rates in AZ 300MiF
Bake Temp Bake Time Develop Rate
200°C 60 sec ~20 nm/min
210°C 60 sec ~3 nm/min
220°C 60 sec ~0.1 nm/min

Courtesy Sean Demura, III-V Innovative Solutions, 2019