Difference between revisions of "Sputtering Recipes"
Jump to navigation
Jump to search
Line 15: | Line 15: | ||
*{{fl|IBD-SiO2-Recipe.pdf|Recipe: SiO{{Sub|2}}_dep}} |
*{{fl|IBD-SiO2-Recipe.pdf|Recipe: SiO{{Sub|2}}_dep}} |
||
− | == |
+ | ==Si<sub>3</sub>N<sub>4</sub> deposition (IBD)== |
* Refractive Index ≈ 2.01 |
* Refractive Index ≈ 2.01 |
||
* Rate ≈ 4.5nm/min (users must calibrate this prior to critical deps) |
* Rate ≈ 4.5nm/min (users must calibrate this prior to critical deps) |
Revision as of 13:12, 13 August 2013
Back to Vacuum Deposition Recipes.
Sputter 1 (Custom)
Sputter 2 (SFI Endeavor)
Sputter 3 (AJA ATC 2000-F)
Sputter 4 (AJA ATC 2200-V)
Sputter 5 (Lesker AXXIS)
Ion Beam Deposition (Veeco NEXUS)
IBD Calibrations Spreadsheet - Records of historical film depositions (rates, indices), Uniformity etc. All users are required to enter their calibration deps (simple test deps only)
SiO2 deposition (IBD)
- Refractive Index: ≈1.485
- Rate: ≈6.1nm/min (users must calibrate this prior to critical deps)
- Stress ≈ -320MPa (compressive)
Si3N4 deposition (IBD)
- Refractive Index ≈ 2.01
- Rate ≈ 4.5nm/min (users must calibrate this prior to critical deps)
- Stress ≈ -1756MPa (compressive)
Ta2O5 deposition (IBD)
- Refractive Index ≈ 2.10
- Rate ≈7.8nm/min (users must calibrate this prior to critical deps)
- Stress ≈ -140MPa (compressive)
TiO2 deposition (IBD)
- Refractive Index ≈ 2.3-2.4
- Dep Rate ≈ 1.8nm/min
- Recipe: TiO2_dep