Difference between revisions of "Test Data of etching SiO2 with CHF3/CF4/O2 (using this recipe only for Fluorine etch of the underneath layer)"
Jump to navigation
Jump to search
(add data) |
|||
Line 13: | Line 13: | ||
|0.74 |
|0.74 |
||
|77.9 |
|77.9 |
||
+ | |- |
||
+ | |1/28/19 |
||
+ | |I21902 |
||
+ | |92.1 |
||
+ | |0.77 |
||
+ | | |
||
|} |
|} |
||
https://www.nanotech.ucsb.edu/wiki/images/f/f1/SiO2_Etch_using_ICP2_with_O2.pdf |
https://www.nanotech.ucsb.edu/wiki/images/f/f1/SiO2_Etch_using_ICP2_with_O2.pdf |
Revision as of 10:37, 29 January 2019
ICP#2: 0.5Pa, 50/500W, CHF3/CF4/O2=35/5/10sccm, time=210 sec | ||||
Date | Sample# | Etch Rate (nm/min) | Etch Selectivity (SiO2/PR) | Averaged Sidewall Angle (o) |
10/5/2018 | SiO2#01 | 95.2 | 0.74 | 77.9 |
1/28/19 | I21902 | 92.1 | 0.77 |
https://www.nanotech.ucsb.edu/wiki/images/f/f1/SiO2_Etch_using_ICP2_with_O2.pdf