Difference between revisions of "Vacuum Deposition Recipes"

From UCSB Nanofab Wiki
Jump to navigation Jump to search
(Corrected Unaxis Dep links. New row: low-stress Nitride.)
m (→‎Process Control Data: smaller font)
 
(13 intermediate revisions by 3 users not shown)
Line 1: Line 1:
  +
===[[Process Group - Process Control Data#Deposition .28Process Control Data.29|<u>Process Control Data</u>]]===
{{Recipe Table Explanation}}
 
  +
<small>''See [[Process Group - Process Control Data#Deposition .28Process Control Data.29|linked page]] for process control data (calibration data over time, such as dep. rate, refractive index, stress etc.) over time, for a selection of highly used tools/films.''</small>
  +
  +
===Deposition Tools/Materials Table===
  +
  +
*<small>'''R''': ''Recipe is available. Clicking this link will take you to the recipe.''</small>
  +
*<small>'''A''': ''Material is available for use, but no recipes are provided.''</small>
  +
 
{| class="wikitable" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center;" border="1"
 
{| class="wikitable" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center;" border="1"
 
|- bgcolor="#d0e7ff"
 
|- bgcolor="#d0e7ff"
Line 19: Line 26:
 
| width="65" bgcolor="#daf1ff" |[[Sputtering_Recipes#Sputter_3_.28AJA_ATC_2000-F.29|Sputter 3<br>(AJA ATC 2000-F)]]
 
| width="65" bgcolor="#daf1ff" |[[Sputtering_Recipes#Sputter_3_.28AJA_ATC_2000-F.29|Sputter 3<br>(AJA ATC 2000-F)]]
 
| width="65" bgcolor="#daf1ff" |[[Sputtering_Recipes#Sputter_4_.28AJA_ATC_2200-V.29|Sputter 4<br>(AJA ATC 2200-V)]]
 
| width="65" bgcolor="#daf1ff" |[[Sputtering_Recipes#Sputter_4_.28AJA_ATC_2200-V.29|Sputter 4<br>(AJA ATC 2200-V)]]
| width="65" bgcolor="#daf1ff" |[https://wiki.nanotech.ucsb.edu/wiki/index.php/Sputtering_Recipes#Sputter_5_.28AJA_ATC_2200-V.29 Sputter 5 (AJA ATC 2200-V)]
+
| width="65" bgcolor="#daf1ff" |[https://wiki.nanotech.ucsb.edu/w/index.php?title=Sputtering_Recipes#Sputter_5_.28AJA_ATC_2200-V.29 Sputter 5 (AJA ATC 2200-V)]
 
| width="55" bgcolor="#daf1ff" |[[Sputtering_Recipes#Ion_Beam_Deposition_.28Veeco_NEXUS.29|Ion Beam<br>Deposition (Veeco Nexus)]]
 
| width="55" bgcolor="#daf1ff" |[[Sputtering_Recipes#Ion_Beam_Deposition_.28Veeco_NEXUS.29|Ion Beam<br>Deposition (Veeco Nexus)]]
 
| width="45" bgcolor="#daf1ff" |[[Thermal Evaporation Recipes#Thermal_Evap_1|Thermal<br>Evap 1]]
 
| width="45" bgcolor="#daf1ff" |[[Thermal Evaporation Recipes#Thermal_Evap_1|Thermal<br>Evap 1]]
Line 71: Line 78:
 
| bgcolor="#eeffff" |{{rl|Sputtering Recipes|Al2O3 Deposition (Sputter 4)}}
 
| bgcolor="#eeffff" |{{rl|Sputtering Recipes|Al2O3 Deposition (Sputter 4)}}
 
| bgcolor="#eeffff" |<br>
 
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |[https://wiki.nanotech.ucsb.edu/wiki/index.php/Sputtering_Recipes#Al2O3_deposition_.28IBD.29 R]
+
| bgcolor="#eeffff" |[https://wiki.nanotech.ucsb.edu/w/index.php?title=Sputtering_Recipes#Al2O3_deposition_.28IBD.29 R]
 
| bgcolor="#eeffff" |<br>
 
| bgcolor="#eeffff" |<br>
 
| bgcolor="#eeffff" |<br>
 
| bgcolor="#eeffff" |<br>
Line 187: Line 194:
 
|<br>
 
|<br>
 
|{{Al/E4}}
 
|{{Al/E4}}
|[https://wiki.nanotech.ucsb.edu/wiki/index.php/Sputtering_Recipes#Sputter_3_.28AJA_ATC_2000-F.29 R]
+
|[https://wiki.nanotech.ucsb.edu/w/index.php?title=Sputtering_Recipes#Sputter_3_.28AJA_ATC_2000-F.29 R]
 
|<br>
 
|<br>
 
|<br>
 
|<br>
Line 529: Line 536:
 
| bgcolor="#eeffff" |[[Sputtering Recipes|A]]
 
| bgcolor="#eeffff" |[[Sputtering Recipes|A]]
 
| bgcolor="#eeffff" |{{rl|Sputtering Recipes|Sputter 4 (AJA ATC 2200-V)}}
 
| bgcolor="#eeffff" |{{rl|Sputtering Recipes|Sputter 4 (AJA ATC 2200-V)}}
| bcolor="EEFFFF" |<br>
+
| bcolor="EEFFFF" |{{rl|Sputtering Recipes|Sputter 5 (AJA ATC 2200-V)}}
 
| bgcolor="#eeffff" |<br>
 
| bgcolor="#eeffff" |<br>
 
| bgcolor="#eeffff" |<br>
 
| bgcolor="#eeffff" |<br>
Line 545: Line 552:
 
|{{Al/E4}}
 
|{{Al/E4}}
 
|<br>
 
|<br>
  +
|[[Sputtering Recipes#Ru Deposition .28Sputter 4.29|R]]
|<br>
 
 
|<br>
 
|<br>
 
|<br>
 
|<br>
Line 568: Line 575:
 
| bgcolor="#eeffff" |<br>
 
| bgcolor="#eeffff" |<br>
 
| bgcolor="#eeffff" |<br>
 
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |[https://wiki.nanotech.ucsb.edu/wiki/index.php/PECVD_Recipes#Amorphous-Si_deposition_.28PECVD_.232.29 R]
+
| bgcolor="#eeffff" |[https://wiki.nanotech.ucsb.edu/w/index.php?title=PECVD_Recipes#Amorphous-Si_deposition_.28PECVD_.232.29 R]
 
| bgcolor="#eeffff" |
 
| bgcolor="#eeffff" |
 
| bgcolor="#eeffff" |<br>
 
| bgcolor="#eeffff" |<br>
Line 590: Line 597:
 
|<br>
 
|<br>
 
|-
 
|-
!SiN - Low Stress
+
! bgcolor="#d0e7ff" align="center" |SiN - Low Stress
  +
|
!
 
  +
|
!
 
  +
|
!
 
  +
|
!
 
  +
|
!
 
  +
|
!
 
  +
|
!
 
  +
|
!
 
  +
|
!
 
  +
|
!
 
!{{rl|PECVD Recipes|Low-Stress SiN - LS-SiN (PECVD#1)}}
+
|{{rl|PECVD Recipes|Low-Stress SiN - LS-SiN (PECVD#1)}}
!{{rl|PECVD Recipes|Low-Stress SiN deposition (PECVD #2)}}
+
|{{rl|PECVD Recipes|Low-Stress SiN deposition (PECVD #2)}}
!{{rl|PECVD Recipes|SiN LS 250C Deposition (Unaxis VLR)}}
+
|{{rl|PECVD Recipes|SiN LS 250C Deposition (Unaxis VLR)}}
  +
|
!
 
  +
|
!
 
 
|-
 
|-
 
! bgcolor="#d0e7ff" align="center" |SiO<sub>2</sub>
 
! bgcolor="#d0e7ff" align="center" |SiO<sub>2</sub>
Line 632: Line 639:
 
|<br>
 
|<br>
 
|<br>
 
|<br>
|[https://wiki.nanotech.ucsb.edu/wiki/index.php/Sputtering_Recipes#SiOxNy_deposition_.28IBD.29 A]
+
|[https://wiki.nanotech.ucsb.edu/w/index.php?title=Sputtering_Recipes#SiOxNy_deposition_.28IBD.29 R]
 
|<br>
 
|<br>
 
|<br>
 
|<br>
Line 716: Line 723:
 
| bgcolor="#eeffff" |{{rl|Sputtering Recipes|Sputter 3 (AJA ATC 2000-F)}}
 
| bgcolor="#eeffff" |{{rl|Sputtering Recipes|Sputter 3 (AJA ATC 2000-F)}}
 
| bgcolor="#eeffff" |{{rl|Sputtering Recipes|Ti-Au Deposition (Sputter 4)}}
 
| bgcolor="#eeffff" |{{rl|Sputtering Recipes|Ti-Au Deposition (Sputter 4)}}
| bgcolor="#eeffff" |<br>
+
| bgcolor="#eeffff" |{{rl|Sputtering Recipes|Sputter 5 (AJA ATC 2200-V)}}
 
| bgcolor="#eeffff" |<br>[[Sputtering_Recipes#Ion_Beam_Deposition_.28Veeco_NEXUS.29|A]]
 
| bgcolor="#eeffff" |<br>[[Sputtering_Recipes#Ion_Beam_Deposition_.28Veeco_NEXUS.29|A]]
 
| bgcolor="#eeffff" |<br>
 
| bgcolor="#eeffff" |<br>
Line 732: Line 739:
 
|<br>
 
|<br>
 
|<br>
 
|<br>
|[https://wiki.nanotech.ucsb.edu/wiki/index.php/Sputtering_Recipes#Sputter_4_.28AJA_ATC_2200-V.29 R]
+
|[https://wiki.nanotech.ucsb.edu/w/index.php?title=Sputtering_Recipes#Sputter_4_.28AJA_ATC_2200-V.29 R]
 
|<br>
 
|<br>
 
|[[Sputtering_Recipes#Ion_Beam_Deposition_.28Veeco_NEXUS.29|A]]
 
|[[Sputtering_Recipes#Ion_Beam_Deposition_.28Veeco_NEXUS.29|A]]

Latest revision as of 15:44, 7 July 2022

Process Control Data

See linked page for process control data (calibration data over time, such as dep. rate, refractive index, stress etc.) over time, for a selection of highly used tools/films.

Deposition Tools/Materials Table

  • R: Recipe is available. Clicking this link will take you to the recipe.
  • A: Material is available for use, but no recipes are provided.
Vacuum Deposition Recipes

E-Beam Evaporation Sputtering Thermal Evaporation Plasma Enhanced Chemical
Vapor Deposition (PECVD)
Atomic Layer Deposition Molecular Vapor Deposition
Material E-Beam 1 (Sharon) E-Beam 2 (Custom) E-Beam 3 (Temescal) E-Beam 4 (CHA) Sputter 3
(AJA ATC 2000-F)
Sputter 4
(AJA ATC 2200-V)
Sputter 5 (AJA ATC 2200-V) Ion Beam
Deposition (Veeco Nexus)
Thermal
Evap 1
Thermal Evap 2 (Solder) PECVD 1
(PlasmaTherm 790)
PECVD 2
(Advanced Vacuum)
Unaxis VLR ICP-PECVD Atomic Layer Deposition (Oxford FlexAL) Molecular Vapor Deposition (Tool)
Ag A
A A A A








Al A
A A A R

A
A A




Al2O3 A A

A R
R




R
AlN



A A
A




R
Au A
A A A R

A A




B














C R
CeO2
R












Co A

A R









Cr A

A R


A A




Cu A


R A








Fe A

A R









Ge A
A A A A








GeO2 A
Gd A

A










Hf A













HfO2



A A






R
In








A




Ir A













ITO
R

A A
A






MgF2 A A
MgO A
Mo A


R A








Nb A



R








Nd



A








Ni A
A A R


A A




NiCr A A
NiFe A A A
Pd A
A A



A A




Pt A
A A A R R





R
Ru A

A
R






R
Si
A

R A

A



R

SiN



R A
R

R R R

SiN - Low Stress R R R
SiO2 A A

R A A R

R R R R
SiOxNy






R

R



Sn








A




SrF2
A












Ta A


R A

A







Ta2O5


A


R






Ti A
A A R R R
A







TiN




R
A




R
TiW A


A R








TiO2
A

A R
R




R
V



A A








W A


A R








Zn







A A




ZnO












R
Zr A

A A A








ZrO2












R
Material E-Beam 1 (Sharon) E-Beam 2 (Custom) E-Beam 3 (Temescal) E-Beam 4 (CHA) Sputter 3
(ATC 2000-F)
Sputter 4
(ATC 2200-V)
Sputter 5 (ATC 2200-V) Ion Beam
Deposition (Veeco Nexus)
Thermal
Evap 1
Thermal Evap 2 (Solder) PECVD 1
(PlasmaTherm 790)
PECVD 2
(Advanced Vacuum)
Unaxis VLR ICP-PECVD Atomic Layer Deposition (Oxford FlexAl) Molecular Vapor Deposition (Tool)