Test Data of etching SiO2 with CHF3/CF4/O2 (using this recipe only for Fluorine etch of the underneath layer)

From UCSB Nanofab Wiki
Jump to navigation Jump to search
The printable version is no longer supported and may have rendering errors. Please update your browser bookmarks and please use the default browser print function instead.
ICP#2: 0.5Pa, 50/500W, CHF3/CF4/O2=35/5/10sccm, time=210 sec
Date Sample# Etch Rate (nm/min) Etch Selectivity (SiO2/PR) Averaged Sidewall Angle (o) SEM Images
10/5/2018 SiO2#01 95.2 0.74 77.9 [1]
1/28/2019 I21902 92.1 0.77 [2]
3/6/2019 I21903 88.5 0.80 79.4 [3]
7/12/2019 I21906 91.9 0.69 78.1 [4]