Difference between revisions of "Test Data of Etching SiO2 with CHF3/CF4-Fluorine ICP Etcher"

From UCSB Nanofab Wiki
Jump to navigation Jump to search
m (fixed typo)
m (added entry to FL cals)
Line 12: Line 12:
 
|Observations/Notes
 
|Observations/Notes
 
|SEM Images (45d, cross section)
 
|SEM Images (45d, cross section)
 +
|-
 +
|4/26/22
 +
|NP_SiO2_Fl_08
 +
|344.7
 +
|
 +
|
 +
|
 +
|[https://wiki.nanotech.ucsb.edu/w/images/c/c2/SiO2_Fl_08_45D_004.jpg <nowiki>[1]</nowiki>] [https://wiki.nanotech.ucsb.edu/w/images/4/47/SiO2_Fl_08_CS_005.jpg <nowiki>[2]</nowiki>]
 
|-
 
|-
 
|4/20/22
 
|4/20/22
Line 29: Line 37:
 
|[https://wiki.nanotech.ucsb.edu/w/images/7/70/SiO2_Fl_06_45D_002.jpg <nowiki>[1]</nowiki>] [https://wiki.nanotech.ucsb.edu/w/images/6/68/SiO2_Fl_06_CS_002.jpg <nowiki>[2]</nowiki>]
 
|[https://wiki.nanotech.ucsb.edu/w/images/7/70/SiO2_Fl_06_45D_002.jpg <nowiki>[1]</nowiki>] [https://wiki.nanotech.ucsb.edu/w/images/6/68/SiO2_Fl_06_CS_002.jpg <nowiki>[2]</nowiki>]
 
|-
 
|-
|3/29/2022
+
|3/29/22
 
|NP_SiO2_Fl_05
 
|NP_SiO2_Fl_05
 
|334.7
 
|334.7

Revision as of 09:09, 4 May 2022

  This page is under construction - we are in the process of standardizing and collecting process control data for this tool.  -- Demis 2022-02-11


Fluorine ICP: 3.8mT, 50/900W, CHF3/CF4=10/30sccm, time=90 sec
Date Sample # Etch Rate (nm/min) Etch Selectivity (SiO2/PR) Averaged Sidewalls Angle Observations/Notes SEM Images (45d, cross section)
4/26/22 NP_SiO2_Fl_08 344.7 [1] [2]
4/20/22 NP_SiO2_Fl_07 354.7 [1] [2]
4/14/22 NP_SiO2_Fl_06 352.7 *need to measure PR [1] [2]
3/29/22 NP_SiO2_Fl_05 334.7 1.07 [1][2]
3/09/22 NP_SiO2_Fl_04 358.9 1.06 [1] [2]
3/02/22 NP_SiO2_Fl_03 347 1.05 [1] [2]
2/23/22 NP_SiO2_Fl_02 362.7 1.02 [1] [2]


Fluorine ICP: 3.8mT, 50/900W, CHF3/CF4=10/30sccm, time=210 sec'
Date Sample# Etch Rate (nm/min) Etch Selectivity (SiO2/PR) Averaged Sidewall Angle (o) Observations/Notes SEM Image
11/5/2021 SOFL01 136 1.2 [1]
02/09/22 NP_SiO2_Fl_01 Etched for 210s, all of PR was etched off [1]


Fluorine ICP: 3.8mT, 50/800W, CHF3/CF4=10/30sccm, time=90 sec
Date Sample# Etch Rate (nm/min) Etch Selectivity (SiO2/PR) Averaged Sidewall Angle (o) Notes/Observations SEM Images
1/28/2021 FE2102 309 0.99 [2]