Difference between revisions of "Test Data of Etching SiO2 with CHF3/CF4-Fluorine ICP Etcher"
Jump to navigation
Jump to search
(moved cals table to the top) |
|||
(25 intermediate revisions by 3 users not shown) | |||
Line 1: | Line 1: | ||
− | '''''This page is under construction - we are in the process of standardizing and collecting process control data for this tool. -- Demis 2022-02-11''''' |
||
− | |||
{| class="wikitable" |
{| class="wikitable" |
||
− | | colspan=" |
+ | | colspan="7" |Fluorine ICP: 3.8mT, 50/'''900W''', CHF3/CF4=10/30sccm, time='''90 sec''' |
− | | |
||
|- |
|- |
||
|Date |
|Date |
||
− | |Sample# |
+ | |Sample # |
− | |Etch |
+ | |Etch Rate (nm/min) |
− | |Etch |
+ | |Etch Selectivity (SiO2/PR) |
− | |Averaged |
+ | |Averaged Sidewalls Angle |
|Observations/Notes |
|Observations/Notes |
||
+ | |SEM Images (45d, cross section) |
||
− | |SEM Image |
||
|- |
|- |
||
− | | |
+ | |01/09/23 |
+ | |ND_FL_010923 |
||
− | |SOFL01 |
||
+ | |263.3 |
||
− | |136 |
||
− | |1. |
+ | |1.31 |
| |
| |
||
| |
| |
||
− | |[https://wiki.nanotech.ucsb.edu/w/images/ |
+ | |[https://wiki.nanotech.ucsb.edu/w/images/9/9b/30D_FICP_010923_002.jpg <nowiki>[30D]</nowiki>][https://wiki.nanotech.ucsb.edu/w/images/2/2b/CS_FICP_010923_003.jpg <nowiki>[CS]</nowiki>] |
|- |
|- |
||
− | | |
+ | |12/14/22 |
+ | |ND_FL_121422 |
||
− | |NP_SiO2_Fl_01 |
||
+ | |266.7 |
||
+ | |1.29 |
||
| |
| |
||
| |
| |
||
+ | |[https://wiki.nanotech.ucsb.edu/w/images/6/62/30D_FICP_121422_002.jpg <nowiki>[30D]</nowiki>][https://wiki.nanotech.ucsb.edu/w/images/5/5b/CS_FICP_121422_002.jpg <nowiki>[CS]</nowiki>] |
||
+ | |- |
||
+ | |12/09/22 |
||
+ | |ND_FL_120922 |
||
+ | |260 |
||
+ | |1.26 |
||
| |
| |
||
+ | | |
||
− | |Etched for 210s, all of PR was etched off |
||
− | |[https://wiki.nanotech.ucsb.edu/w/images/ |
+ | |[https://wiki.nanotech.ucsb.edu/w/images/7/72/30D_FICP_120922_002.jpg <nowiki>[30D]</nowiki>][https://wiki.nanotech.ucsb.edu/w/images/4/4e/CS_FICP_120922_002.jpg <nowiki>[CS]</nowiki>] |
− | |} |
||
− | {| class="wikitable" |
||
− | | colspan="7" |Fluorine ICP: 3.8mT, 50/'''900W''', CHF3/CF4=10/30sccm, time='''90 sec''' |
||
|- |
|- |
||
+ | |11/18/22 |
||
− | |Date |
||
+ | |ND_FL_111822 |
||
− | |Sample # |
||
+ | |268 |
||
− | |Etch Rate (nm/min) |
||
+ | |1.01 |
||
− | |Etch Selectivity (SiO2/PR) |
||
+ | | |
||
− | |Averaged Sidewalls Angle |
||
+ | | |
||
− | |Observations/Notes |
||
+ | |[https://wiki.nanotech.ucsb.edu/w/images/6/64/30D_FICP_111822_002.jpg <nowiki>[30D]</nowiki>][https://wiki.nanotech.ucsb.edu/w/images/c/c5/CS_FICP_111822_002.jpg <nowiki>[CS]</nowiki>] |
||
− | |SEM Images (45d, cross section) |
||
|- |
|- |
||
− | | |
+ | |11/07/22 |
+ | |ND_FL_110722 |
||
− | |NP_SiO2_Fl_02 |
||
− | | |
+ | |264.7 |
− | | |
+ | |0.96 |
| |
| |
||
| |
| |
||
− | |[https://wiki.nanotech.ucsb.edu/w/images/c/c8/ |
+ | |[https://wiki.nanotech.ucsb.edu/w/images/c/c8/30D_FICP_110722_002.jpg <nowiki>[30D]</nowiki>] [https://wiki.nanotech.ucsb.edu/w/images/e/e9/CS_FICP_110722_002.jpg <nowiki>[CS]</nowiki>] |
|- |
|- |
||
− | | |
+ | |10/24/22 |
+ | |ND_FL_102422 |
||
− | |NP_SiO2_Fl_03 |
||
+ | |266.7 |
||
− | |~360 - 370 |
||
− | |1. |
+ | |1.22 |
| |
| |
||
| |
| |
||
− | |[https://wiki.nanotech.ucsb.edu/w/images/ |
+ | |[https://wiki.nanotech.ucsb.edu/w/images/3/38/30D_FICP_102422_002.jpg <nowiki>[30D]</nowiki>][https://wiki.nanotech.ucsb.edu/w/images/7/74/CS_FICP_102422_002.jpg <nowiki>[CS]</nowiki>] |
|- |
|- |
||
− | | |
+ | |10/14/22 |
+ | |ND_FL_101422 |
||
− | |NP_SiO2_Fl_04 |
||
+ | |249 |
||
− | |358.9 |
||
− | | |
+ | |0.82 |
| |
| |
||
+ | |Image drifted very slightly |
||
+ | in SEM. May account for |
||
+ | |||
+ | low selectivity. |
||
+ | |[https://wiki.nanotech.ucsb.edu/w/images/7/76/30D_FICP_101422_002.jpg <nowiki>[30D]</nowiki>] [https://wiki.nanotech.ucsb.edu/w/images/c/ca/CS_FICP_101422_003.jpg <nowiki>[CS]</nowiki>] |
||
+ | |- |
||
+ | |10/3/22 |
||
+ | |ND_FL_100322 |
||
+ | |228 |
||
+ | |1.10 |
||
| |
| |
||
+ | |Low etch rate. |
||
− | |[https://wiki.nanotech.ucsb.edu/w/images/f/f3/SiO2_FL_04_45D_001.jpg <nowiki>[1]</nowiki>] [https://wiki.nanotech.ucsb.edu/w/images/d/db/SiO2_Fl_04_CS_005.jpg <nowiki>[2]</nowiki>] |
||
+ | |[https://wiki.nanotech.ucsb.edu/w/images/8/8e/30D_10302022_FICP_002.jpg <nowiki>[30D]</nowiki>] [https://wiki.nanotech.ucsb.edu/w/images/9/92/CS_10302022_FICP_002.jpg <nowiki>[CS]</nowiki>] |
||
+ | |- |
||
+ | |9/12/22 |
||
+ | |ND_FL_091222 |
||
+ | |278 |
||
+ | |1.33 |
||
+ | | |
||
+ | |high selectivity, may be |
||
+ | due to new Si wafer |
||
+ | |[https://wiki.nanotech.ucsb.edu/w/images/8/8e/30D_FICP_091222_002.jpg <nowiki>[30D]</nowiki>] [https://wiki.nanotech.ucsb.edu/w/images/e/e7/CS_FICP_091222_002.jpg <nowiki>[CS]</nowiki>] |
||
+ | |- |
||
+ | |8/26/22 |
||
+ | |ND_FL_082622 |
||
+ | |288 |
||
+ | |0.97 |
||
+ | | |
||
+ | |Low selectivity/e. rate |
||
+ | |[https://wiki.nanotech.ucsb.edu/w/images/b/b9/30D_FICP_082622_001.jpg <nowiki>[30D]</nowiki>] [https://wiki.nanotech.ucsb.edu/w/images/8/86/CS_FICP_082622_001.jpg <nowiki>[CS]</nowiki>] |
||
+ | |- |
||
+ | |8/22/22 |
||
+ | |ND_FL_082222 |
||
+ | |252.7 |
||
+ | |0.93 |
||
+ | | |
||
+ | |Lower selectivity/e. rate |
||
+ | |[https://wiki.nanotech.ucsb.edu/w/images/3/3d/40D_FICP_082222_001.jpg <nowiki>[40D]</nowiki>] [https://wiki.nanotech.ucsb.edu/w/images/5/5b/CS_FICP_082222_002.jpg <nowiki>[CS]</nowiki>] |
||
+ | |- |
||
+ | |8/19/22 |
||
+ | |ND_Fl_081922 |
||
+ | |260.7 |
||
+ | |0.99 |
||
+ | | |
||
+ | |Low selectivity/etch rate |
||
+ | |[https://wiki.nanotech.ucsb.edu/w/images/8/82/30D_08192022_FICP_001.jpg <nowiki>[30D]</nowiki>][https://wiki.nanotech.ucsb.edu/w/images/5/56/CS_08192022_FICP_001.jpg <nowiki>[CS]</nowiki>] |
||
+ | |- |
||
+ | | colspan="7" |'''''Change in operator - SEMs below (by NP) are erroneously measured to the trench, instead of flat plane.''''' |
||
+ | |- |
||
+ | |5/18/22 |
||
+ | |NP_SiO2_Fl_10 |
||
+ | |308.7 |
||
+ | |1.19 |
||
+ | | |
||
+ | |still lower etch rate |
||
+ | |[https://wiki.nanotech.ucsb.edu/w/images/5/5d/SiO2_Fl_10_45D-003.jpg <nowiki>[1]</nowiki>] [https://wiki.nanotech.ucsb.edu/w/images/0/06/SiO2_Fl_10_CS_007.jpg <nowiki>[2]</nowiki>] |
||
+ | |- |
||
+ | |5/10/22 |
||
+ | |NP_SiO2_Fl_09 |
||
+ | |307.3 |
||
+ | |1.15 |
||
+ | | |
||
+ | |*etch rate seems lower* |
||
+ | |[https://wiki.nanotech.ucsb.edu/w/images/a/a8/SiO2_Fl_09_45D_005.jpg <nowiki>[1]</nowiki>] [https://wiki.nanotech.ucsb.edu/w/images/a/a7/SiO2_Fl_09_CS_006.jpg <nowiki>[2]</nowiki>] |
||
+ | |- |
||
+ | |4/26/22 |
||
+ | |NP_SiO2_Fl_08 |
||
+ | |344.7 |
||
+ | |1.4 |
||
+ | | |
||
+ | | |
||
+ | |[https://wiki.nanotech.ucsb.edu/w/images/c/c2/SiO2_Fl_08_45D_004.jpg <nowiki>[1]</nowiki>] [https://wiki.nanotech.ucsb.edu/w/images/4/47/SiO2_Fl_08_CS_005.jpg <nowiki>[2]</nowiki>] |
||
+ | |- |
||
+ | |4/20/22 |
||
+ | |NP_SiO2_Fl_07 |
||
+ | |354.7 |
||
+ | |1.11 |
||
+ | | |
||
+ | | |
||
+ | |[https://wiki.nanotech.ucsb.edu/w/images/f/f5/SiO2_Fl_07_45D_003.jpg <nowiki>[1]</nowiki>] [https://wiki.nanotech.ucsb.edu/w/images/3/34/SiO2_Fl_07_CS_004.jpg <nowiki>[2]</nowiki>] |
||
+ | |- |
||
+ | |4/14/22 |
||
+ | |NP_SiO2_Fl_06 |
||
+ | |352.7 |
||
+ | |1.11 |
||
+ | | |
||
+ | | |
||
+ | |[https://wiki.nanotech.ucsb.edu/w/images/7/70/SiO2_Fl_06_45D_002.jpg <nowiki>[1]</nowiki>] [https://wiki.nanotech.ucsb.edu/w/images/6/68/SiO2_Fl_06_CS_002.jpg <nowiki>[2]</nowiki>] |
||
|- |
|- |
||
− | |3/29/ |
+ | |3/29/22 |
|NP_SiO2_Fl_05 |
|NP_SiO2_Fl_05 |
||
|334.7 |
|334.7 |
||
Line 72: | Line 160: | ||
| |
| |
||
|[https://wiki.nanotech.ucsb.edu/w/images/a/a3/SiO2_Fl_03_45D_002.jpg <nowiki>[1]</nowiki>][https://wiki.nanotech.ucsb.edu/w/images/e/e2/SiO2_Fl_05_CS_002.jpg <nowiki>[2]</nowiki>] |
|[https://wiki.nanotech.ucsb.edu/w/images/a/a3/SiO2_Fl_03_45D_002.jpg <nowiki>[1]</nowiki>][https://wiki.nanotech.ucsb.edu/w/images/e/e2/SiO2_Fl_05_CS_002.jpg <nowiki>[2]</nowiki>] |
||
− | |} |
||
− | |||
− | |||
− | {| class="wikitable" |
||
− | | colspan="7" |Fluorine ICP: 3.8mT, 50/800W, CHF3/CF4=10/30sccm, time=90 sec |
||
|- |
|- |
||
+ | |3/09/22 |
||
− | |Date |
||
+ | |NP_SiO2_Fl_04 |
||
− | |Sample# |
||
+ | |358.9 |
||
− | |Etch Rate (nm/min) |
||
+ | |1.06 |
||
− | |Etch Selectivity (SiO2/PR) |
||
+ | | |
||
− | |Averaged Sidewall Angle (<sup>o</sup>) |
||
+ | | |
||
− | |Notes/Observations |
||
+ | |[https://wiki.nanotech.ucsb.edu/w/images/f/f3/SiO2_FL_04_45D_001.jpg <nowiki>[1]</nowiki>] [https://wiki.nanotech.ucsb.edu/w/images/d/db/SiO2_Fl_04_CS_005.jpg <nowiki>[2]</nowiki>] |
||
− | |SEM Images |
||
|- |
|- |
||
− | | |
+ | |3/02/22 |
+ | |NP_SiO2_Fl_03 |
||
− | |FE2102 |
||
− | | |
+ | |347 |
− | | |
+ | |1.05 |
| |
| |
||
| |
| |
||
− | |[https://wiki.nanotech.ucsb.edu/w/images/ |
+ | |[https://wiki.nanotech.ucsb.edu/w/images/b/b7/SiO2_Fl_03_45D_001.jpg <nowiki>[1]</nowiki>] [https://wiki.nanotech.ucsb.edu/w/images/3/38/SiO2_Fl_03_CS_004.jpg <nowiki>[2]</nowiki>] |
+ | |- |
||
+ | |2/23/22 |
||
+ | |NP_SiO2_Fl_02 |
||
+ | |362.7 |
||
+ | |1.02 |
||
+ | | |
||
+ | | |
||
+ | |[https://wiki.nanotech.ucsb.edu/w/images/c/c8/SiO2_Fl_02_45D_001.jpg <nowiki>[1]</nowiki>] [https://wiki.nanotech.ucsb.edu/w/images/8/89/SiO2_Fl_02_CS_001.jpg <nowiki>[2]</nowiki>] |
||
|} |
|} |
Latest revision as of 15:03, 9 January 2023
Fluorine ICP: 3.8mT, 50/900W, CHF3/CF4=10/30sccm, time=90 sec | ||||||
Date | Sample # | Etch Rate (nm/min) | Etch Selectivity (SiO2/PR) | Averaged Sidewalls Angle | Observations/Notes | SEM Images (45d, cross section) |
01/09/23 | ND_FL_010923 | 263.3 | 1.31 | [30D][CS] | ||
12/14/22 | ND_FL_121422 | 266.7 | 1.29 | [30D][CS] | ||
12/09/22 | ND_FL_120922 | 260 | 1.26 | [30D][CS] | ||
11/18/22 | ND_FL_111822 | 268 | 1.01 | [30D][CS] | ||
11/07/22 | ND_FL_110722 | 264.7 | 0.96 | [30D] [CS] | ||
10/24/22 | ND_FL_102422 | 266.7 | 1.22 | [30D][CS] | ||
10/14/22 | ND_FL_101422 | 249 | 0.82 | Image drifted very slightly
in SEM. May account for low selectivity. |
[30D] [CS] | |
10/3/22 | ND_FL_100322 | 228 | 1.10 | Low etch rate. | [30D] [CS] | |
9/12/22 | ND_FL_091222 | 278 | 1.33 | high selectivity, may be
due to new Si wafer |
[30D] [CS] | |
8/26/22 | ND_FL_082622 | 288 | 0.97 | Low selectivity/e. rate | [30D] [CS] | |
8/22/22 | ND_FL_082222 | 252.7 | 0.93 | Lower selectivity/e. rate | [40D] [CS] | |
8/19/22 | ND_Fl_081922 | 260.7 | 0.99 | Low selectivity/etch rate | [30D][CS] | |
Change in operator - SEMs below (by NP) are erroneously measured to the trench, instead of flat plane. | ||||||
5/18/22 | NP_SiO2_Fl_10 | 308.7 | 1.19 | still lower etch rate | [1] [2] | |
5/10/22 | NP_SiO2_Fl_09 | 307.3 | 1.15 | *etch rate seems lower* | [1] [2] | |
4/26/22 | NP_SiO2_Fl_08 | 344.7 | 1.4 | [1] [2] | ||
4/20/22 | NP_SiO2_Fl_07 | 354.7 | 1.11 | [1] [2] | ||
4/14/22 | NP_SiO2_Fl_06 | 352.7 | 1.11 | [1] [2] | ||
3/29/22 | NP_SiO2_Fl_05 | 334.7 | 1.07 | [1][2] | ||
3/09/22 | NP_SiO2_Fl_04 | 358.9 | 1.06 | [1] [2] | ||
3/02/22 | NP_SiO2_Fl_03 | 347 | 1.05 | [1] [2] | ||
2/23/22 | NP_SiO2_Fl_02 | 362.7 | 1.02 | [1] [2] |