Sample Size Effect on Etch Rate (Oxford ICP Etcher)

We have found that the size of the InP piece loaded (no adhesive, onto Silicon carrier wafer) affects the etch rate, but does not affect the etch profile - ie. etches are still smooth and vertical, but etch rate varies with sample area.

InP Ridge Etch: 60°C, 3mT, 800W/65W, Cl2=18, H2=15, CH4=10sccm, time=5min05sec (305sec)

Silicon carrier, no adhesive.

Date Sample# Sample Size (dimensions, mm) Sample Size (area, mm2) Etch Rate (nm/min) Etch Selectivity (InP/SiO2) Comments SEM Images
1/11/22 DJ_InPRidge 4.5 x 2.5 11.25 602 64.6nm left ~50% SiO2 masking (GCA Calibration pattern) [1]
1/12/22 DJ_InPRidge 4.5 x 3 13.5 563 76.4nm left ~50% SiO2 masking (GCA Calibration pattern) [2]
1/12/22 DJ_InP#3 4.5 x 3 13.5 612 71nm left ~50% SiO2 masking (GCA Calibration pattern) [3]
1/26/22 NP_? 10 x 10 100 400-450 ~250nm left ~30-40% SiO2 masking (NingC's pattern)
1/26/22 NP_? 1/4 of 50mm wafer 490 378 276nm left ~30-40% SiO2 masking (NingC's pattern) [1]