Difference between revisions of "Lift-Off with DUV Imaging + PMGI Underlayer"
(Acknowledge development by demis) |
(corrected typo) |
||
(12 intermediate revisions by 2 users not shown) | |||
Line 1: | Line 1: | ||
Developed by Demis D. John, ~2017-2019 |
Developed by Demis D. John, ~2017-2019 |
||
This process is intended for Deep-UV Exposure on the ASML DUV Stepper. PMGI is used as the underlayer, which is exposed at the same time as the imaging resist. |
This process is intended for Deep-UV Exposure on the ASML DUV Stepper. PMGI is used as the underlayer, which is exposed at the same time as the imaging resist. |
||
− | |||
− | This process uses PMGI SF-5 @ 4krpm, which spins to about 130nm (maximum metal thickness = 130nm/3 ≈ 45nm) and undercuts laterally about 130-140nm (minimum gap between metals = (2 x 140nm) + 30nm ≈ 350nm). |
||
Adjust spin speed or switch to a different PMGI formulation to tailor the underlayer thickness to your desired metal thickness. |
Adjust spin speed or switch to a different PMGI formulation to tailor the underlayer thickness to your desired metal thickness. |
||
==Tips== |
==Tips== |
||
− | Please see our |
+ | Please see our [https://wiki.nanotech.ucsb.edu/w/images/b/bc/Liftoff-Techniques.pdf Bi-Layer Lift-Off Tutorial] to understand the limitations and requirements for good lift-off. |
*Remember that gaps in between adjacent metal traces can lift-off during the develop! |
*Remember that gaps in between adjacent metal traces can lift-off during the develop! |
||
− | *Need underlayer thickness 2x |
+ | *Need underlayer thickness approx. 2x the desired metal thickness. |
*The underlayer will develop laterally from both sides which can lift-off the imaging resist, so: |
*The underlayer will develop laterally from both sides which can lift-off the imaging resist, so: |
||
− | **Minimum gap between adjacent metals should then be: |
+ | **Minimum gap between adjacent metals should then be: ''greater than 0.5 * underlayer thickness'' |
**Want at least 30-50nm of underlayer width left to support the imaging resist, so the PR doesn't fall over/collapse. |
**Want at least 30-50nm of underlayer width left to support the imaging resist, so the PR doesn't fall over/collapse. |
||
− | *Make sure to use a vertical evaporation - EBeam4 or EBeam1. EBeam3 is not vertical. |
+ | *Make sure to use a vertical evaporation line-of-sight such as [[E-Beam 4 (CHA)|EBeam4]] or [[E-Beam 1 (Sharon)|EBeam1]]. [[E-Beam 3 (Temescal)|EBeam3]] is not vertical unless special care is taken. |
+ | |||
+ | ===Process Limits=== |
||
+ | This process is written with PMGI SF-5 @ 4krpm, which spins to about 130nm |
||
+ | |||
+ | *<u>Maximum metal thickness</u> = 130nm/2 ≈ '''65nm''' (can possibly increase up to 130nm* 2/3 ≈ 85nm) |
||
+ | *Undercuts laterally about 130-140nm, so <u>minimum gap between metals</u> = (2 x 140nm) + ~30nm ≈ '''350nm''' |
||
+ | |||
+ | Adjust the PMGI layer thickness to adjust these process limits. |
||
+ | |||
+ | PMGI could be spun thicker, or double-spun to get thicker underlayers (develop time & undercut will increase accordingly). |
||
+ | PMGI underlayer could be replaced with LOL1000/LOL2000, or another developable underlayer. |
||
==Suggested Process for Liftoff== |
==Suggested Process for Liftoff== |
||
+ | {| class="wikitable" |
||
+ | |De-H2O Bake (eg. 220°C, 1m+) |
||
+ | - or - |
||
+ | Technics O2 ash (300mT, 100W), 15sec |
||
⚫ | |||
+ | |- |
||
⚫ | |||
+ | | |
||
+ | |- |
||
⚫ | |||
+ | | |
||
+ | |- |
||
⚫ | |||
+ | |Can just place wafer directly onto hotplate surface. |
||
+ | Optionally can use lift-pins & Recipe "'''00 220deg, 3min Vac'''"; |
||
+ | --> To prevent wafer sliding: Enable Vacuum with overhead valve, only for wafer landing and then turn off. |
||
⚫ | |||
+ | |- |
||
⚫ | |||
⚫ | |||
⚫ | |||
+ | | |
||
− | *PMGI-Bake: 220°C, 3min (BrewerSci lift-pin hotplate). Can just place wafer directly onto hotplate surface. Optionally can use lift-pins & Recipe "'''''00 220deg, 3min Vac'''''"; Enable Vacuum with overhead valve, only for wafer landing and then turn off to prevent sliding. |
||
+ | |- |
||
⚫ | |||
− | + | |POLOS underside clean: 2000rpm, ACE/ISO/N2 |
|
+ | | |
||
⚫ | |||
+ | |- |
||
⚫ | |||
⚫ | |||
⚫ | |||
+ | | |
||
⚫ | |||
+ | |- |
||
⚫ | |||
⚫ | |||
⚫ | |||
+ | | |
||
⚫ | |||
+ | |- |
||
⚫ | |||
⚫ | |||
⚫ | |||
+ | | |
||
⚫ | |||
+ | |- |
||
⚫ | |||
⚫ | |||
⚫ | |||
⚫ | |||
⚫ | |||
+ | |- |
||
+ | |PEB = 135°C, 1.5min (built-in hotplate) |
||
+ | | |
||
+ | |- |
||
⚫ | |||
⚫ | |||
⚫ | |||
+ | |- |
||
+ | |DI rinse |
||
⚫ | |||
+ | |- |
||
+ | |PEii Technics O2: 30sec (100W/300mT) |
||
⚫ | |||
+ | |- |
||
+ | |'''<u>Metal Evaporation</u>''' |
||
+ | (insert steps) |
||
⚫ | |||
+ | |- |
||
+ | |'''<u>Lift-off in NMP</u>''' |
||
⚫ | |||
+ | Optional: going directly into continuous Ultrasonic can reduce residual particles. |
||
+ | |} |
||
==Data== |
==Data== |
||
Line 46: | Line 92: | ||
===Images / Examples=== |
===Images / Examples=== |
||
− | [[File:PMGI+UV6 lift-off SEM - 2017-06-30 DJ.png|alt=SEM of PR cross-section|none|thumb|578x578px|SEM of holes in PR with above process. Lateral measurement of undercut is only approximate because circle may not have been cut through the exact diameter.]] |
+ | [[File:PMGI+UV6 lift-off SEM - 2017-06-30 DJ.png|alt=SEM of PR cross-section|none|thumb|578x578px|SEM of holes in PR with above process. Top layer is UV6, 140nm underlayer is PMGI, substrate is Silicon. Lateral measurement of undercut is only approximate because circle may not have been cut through the exact diameter. (Demis D. John, 2017)]] |
<br /> |
<br /> |
Latest revision as of 16:32, 27 April 2022
Developed by Demis D. John, ~2017-2019
This process is intended for Deep-UV Exposure on the ASML DUV Stepper. PMGI is used as the underlayer, which is exposed at the same time as the imaging resist.
Adjust spin speed or switch to a different PMGI formulation to tailor the underlayer thickness to your desired metal thickness.
Tips
Please see our Bi-Layer Lift-Off Tutorial to understand the limitations and requirements for good lift-off.
- Remember that gaps in between adjacent metal traces can lift-off during the develop!
- Need underlayer thickness approx. 2x the desired metal thickness.
- The underlayer will develop laterally from both sides which can lift-off the imaging resist, so:
- Minimum gap between adjacent metals should then be: greater than 0.5 * underlayer thickness
- Want at least 30-50nm of underlayer width left to support the imaging resist, so the PR doesn't fall over/collapse.
- Make sure to use a vertical evaporation line-of-sight such as EBeam4 or EBeam1. EBeam3 is not vertical unless special care is taken.
Process Limits
This process is written with PMGI SF-5 @ 4krpm, which spins to about 130nm
- Maximum metal thickness = 130nm/2 ≈ 65nm (can possibly increase up to 130nm* 2/3 ≈ 85nm)
- Undercuts laterally about 130-140nm, so minimum gap between metals = (2 x 140nm) + ~30nm ≈ 350nm
Adjust the PMGI layer thickness to adjust these process limits.
PMGI could be spun thicker, or double-spun to get thicker underlayers (develop time & undercut will increase accordingly).
PMGI underlayer could be replaced with LOL1000/LOL2000, or another developable underlayer.
Suggested Process for Liftoff
De-H2O Bake (eg. 220°C, 1m+)
- or - Technics O2 ash (300mT, 100W), 15sec |
Oxygen ash is faster and more effective |
Spin PMGI SF-5 @ 4krpm (rcp 7) | |
POLOS underside clean: 2000rpm, ACE/ISO/N2 | |
PMGI-Bake: 220°C, 3min (BrewerSci lift-pin hotplate). | Can just place wafer directly onto hotplate surface.
Optionally can use lift-pins & Recipe "00 220deg, 3min Vac"; --> To prevent wafer sliding: Enable Vacuum with overhead valve, only for wafer landing and then turn off. |
Spin UV-6-0.8 @ rcp 6 (3.5krpm) | |
POLOS underside clean: 2000rpm, ACE/ISO/N2 | |
Soft-Bake = 135°C, 1min (builtin hotplate) | |
(check underside for particulates) | |
ASML Exposure | |
Default: Exp = 37.5mJ // foc = –0.10 | Try this exposure dose but might need to do a FocArray (smaller Image Distribution eg. 5x5) to find proper exposure. |
PEB = 135°C, 1.5min (built-in hotplate) | |
Dev (300MiF) = 50sec (CRITICAL time) | Use cassette & H2O rinse dish prepared
--> not stirring, instead very slow/gentle lift/drop at various angles or gentle swish just to mix developer slightly. |
DI rinse | Very Gently! Dunk into prepared DI dish, and dump/fill gently 2x. Don’t allow direct hard water to hit PR surface. |
PEii Technics O2: 30sec (100W/300mT) | May increase feature size openings by ~50nm. |
Metal Evaporation
(insert steps) |
EBeam#4 or EBeam#1 with vertical/4-inch holders (not planetary) |
Lift-off in NMP | Facing down or vertical.
Optional: going directly into continuous Ultrasonic can reduce residual particles. |
Data
• For PMGI Baked at 220°C for 3min, the PMGI dissolves in AZ 300MIF at a rate of approximately ~600nm/min.
Images / Examples