Difference between revisions of "KLA Tencor P7 - Basic profile instructions"

From UCSB Nanofab Wiki
Jump to navigation Jump to search
m (explain autromatic cals)
m (spelling error)
 
(One intermediate revision by the same user not shown)
Line 1: Line 1:
 
'''KLA Tencor P-7 Profiler Operating Instructions'''
 
'''KLA Tencor P-7 Profiler Operating Instructions'''
   
Note: If the stage is not in the load/unload position, click on ''Sample'' from the top menu bar and select ''Manual Load''. The system periodically performs automatic calibration and does not move back to the Load/Unload position afterwards.
 
   
 
'''Do not open the door if the stage is moving or not at the load/unload position.'''
 
'''Do not open the door if the stage is moving or not at the load/unload position.'''
  +
# Open door and place sample in the center of the chuck.
 
  +
'''Do not run the stylus faster than 10um/s without prior staff approval.'''
# Turn on vacuum and close door.
 
  +
# Click on sample from the top menu bar and select manual load. Visuallyverify the sample is under the stylus. If it is not, unload and reposition sample.
 
  +
'''Do not save changes to generic user recipes.'''
# From the main Profiler screen, select scan recipe.
 
  +
# Single click a scan recipe based on the total height of the structure to be measured.
 
  +
'''Do not reach inside the tool with your hands (tweezers only).'''
# Select the xy icon.
 
  +
# Select Focus. This will lower the stylus and focus on the sample.
 
  +
'''Do not measure step heights greater than 440um from low to high.'''
# Use the arrow buttons on the screen to center sample measurement area. You can also double click on the area to be scanned to center it.
 
  +
# Drag the blue cursor left to right or right to left across feature to be profiled. The arrow shows the scan direction and length of scan.
 
  +
<br />
# Select start. Note: The image will shift down during the scan.
 
  +
# When scan trace appears, select level. Move leveling cursors to flat area and select level again.
 
 
#Open door and place sample in the center of the chuck.
# Measurement cursors will appear. Move cursors to desired locations.
 
 
#Turn on vacuum and close door.
# Read the St Height in microns.
 
 
#Click on sample from the top menu bar and select manual load. Visually verify the sample is under the stylus. If it is not, unload and reposition sample.
# Close window or save data or export graph if needed.
 
 
#From the main Profiler screen, select scan recipe.
# Select Sample from main menu bar.
 
 
#Single click a scan recipe based on the total height of the structure to be measured.
# Select manual load.
 
 
#Select the xy icon.
# Wait for stage to finish moving to load/unload position, open door and switch off vacuum.
 
 
#Select Focus. This will lower the stylus and focus on the sample.
# Remove sample and close door.
 
 
#Use the arrow buttons on the screen to center sample measurement area. You can also double click on the area to be scanned to center it.
 
#Drag the blue cursor left to right or right to left across feature to be profiled. The arrow shows the scan direction and length of scan.
 
#Select start. Note: The image will shift down during the scan.
 
#When scan trace appears, select level. Move leveling cursors to flat area and select level again.
 
#Measurement cursors will appear. Move cursors to desired locations.
 
#Read the St Height in microns.
 
#Close window or save data or export graph if needed.
 
#Select Sample from main menu bar.
 
#Select manual load.
 
#Wait for stage to finish moving to load/unload position, open door and switch off vacuum.
 
#Remove sample and close door.
  +
#Fill out the log-book.
  +
  +
 
Note: If the stage is not in the load/unload position, click on ''Sample'' from the top menu bar and select ''Manual Load''. The system periodically performs automatic calibration and does not move back to the Load/Unload position afterwards.

Latest revision as of 15:20, 2 November 2022

KLA Tencor P-7 Profiler Operating Instructions


Do not open the door if the stage is moving or not at the load/unload position.

Do not run the stylus faster than 10um/s without prior staff approval.

Do not save changes to generic user recipes.

Do not reach inside the tool with your hands (tweezers only).

Do not measure step heights greater than 440um from low to high.


  1. Open door and place sample in the center of the chuck.
  2. Turn on vacuum and close door.
  3. Click on sample from the top menu bar and select manual load. Visually verify the sample is under the stylus. If it is not, unload and reposition sample.
  4. From the main Profiler screen, select scan recipe.
  5. Single click a scan recipe based on the total height of the structure to be measured.
  6. Select the xy icon.
  7. Select Focus. This will lower the stylus and focus on the sample.
  8. Use the arrow buttons on the screen to center sample measurement area. You can also double click on the area to be scanned to center it.
  9. Drag the blue cursor left to right or right to left across feature to be profiled. The arrow shows the scan direction and length of scan.
  10. Select start. Note: The image will shift down during the scan.
  11. When scan trace appears, select level. Move leveling cursors to flat area and select level again.
  12. Measurement cursors will appear. Move cursors to desired locations.
  13. Read the St Height in microns.
  14. Close window or save data or export graph if needed.
  15. Select Sample from main menu bar.
  16. Select manual load.
  17. Wait for stage to finish moving to load/unload position, open door and switch off vacuum.
  18. Remove sample and close door.
  19. Fill out the log-book.


Note: If the stage is not in the load/unload position, click on Sample from the top menu bar and select Manual Load. The system periodically performs automatic calibration and does not move back to the Load/Unload position afterwards.