Filmetrics F40-UV Microscope-Mounted

From UCSB Nanofab Wiki
Jump to navigation Jump to search
The printable version is no longer supported and may have rendering errors. Please update your browser bookmarks and please use the default browser print function instead.
Filmetrics F40-UV Microscope-Mounted
Filmetrics F40-UV - system pic 01.jpg
Location Bay #4
Tool Type Inspection, Test and Characterization
Manufacturer Filmetrics Inc.
Model F40-UV
Description Microscope-mounted optical reflectometry

Primary Supervisor Aidan Hopkins
(805) 893-2343
hopkins@ece.ucsb.edu

Secondary Supervisor

Demis D. John


Recipes N/A


About

The Filmetrics F40-UV is a microscope-mounted thin-film measurement system, allowing you to non-destructively measure thin-film thicknesses in small (patterned) areas on your sample. The microscope is a standard Olympus BHJML metallurgical trinocular microscope. It is an optical reflectometer, acquiring reflection spectra between 400-900nm optical wavelengths (Vis to Near-IR) with a regular halogen microscope light source. The Filmetrics software then performs curve-fitting to determine the thickness and/or refractive index of the measured films.

Capabilities

  • Measure optically transparent thin-films down to ~30nm thickness.
  • Microscope Objectives: 10x, 20x, 50x, 100x, 150x
    • Can measure thin-films in few-micron spot.
  • Acquire Optical Reflection Spectra from 400-900nm
  • Spectrometer/Detector is capable of detecting down to UV ~190nm, but light source does not support this wavelength.
  • Reflectivity curve-fitting for thin-film thickness analysis, supporting many common materials (Si3N4, SiO2 dielectrics, Si, GaAs, InP semiconductors, metals, photoresists etc.)
  • Approx ≥20nm film transparent measurement up to tens of microns.

Operating Procedures

Examples

Good Curve-Fitting

Do not believe your thickness measurements unless the red/blue curves show a reasonably good match!

example spectrum curve fit
Screenshot showing 10x microscope view and optical spectrum/curve fitting of the SiO2 film thickness on top of Platinum contact metal. This is considered a "reasonable" fit because the curves are very similar, but don't overlay perfectly, giving only reasonable confidence in the reported numbers.
example spectrum curve fit
A good fit should show the Calculated (red) curve overlay on top of the Measured (blue) curve. This is a very good curve-fit and the reported thickness/index should be accurate.

Checking whether a dry etch is complete

The F40-UV is very useful for measuring whether a thin-film has been completely removed during a dry etch. This is similar to using laser monitoring during the etch, except that the microscope enables you to measure inside small patterned areas that a laser monitor spot may not fit inside.

In the following example, we are trying to etch away the SiO2 from on top of a Platinum contact metal. The 20x objective allows us to measure the SiO2 thickness on top of the Platinum as we continue to etch in 1 minute increments, measuring in between etches.

Finally, when the SiO2 has been fully removed, we see that we can't get a good fit between the measured (blue) and simulated (red) data.

Since the Platinum layer is thick enough to be opaque to visible light (>50nm), we just modelled this as SiO2 on top of Platinum, ignoring any other materials below the platinum.

Example Screenshot of incomplete SiO2 etch
Incomplete Dry-Etch, showing some residual SiO2 left. "Goodness of Fit" is close to 1.0 in the results pane, and the red+blue curves match closely so we believe the measurement.
Example screenshot of fully removed SiO2 etch
After re-etching, measurement shows bad fit (red and blue curves), and "Goodness of Fit" = 0 in the results pane. The thickness value shown is not real, and this indicates that the SiO2 film has been fully removed since no parameter can give a good fit.

Other Info

Equip > Characterization > Microscopes - see a list of all our microscopes