Difference between revisions of "Dry Etching Recipes"
Jump to navigation
Jump to search
m (fix ICP1 GaAs link) |
m (fix incorrect color header cell) |
||
(29 intermediate revisions by 5 users not shown) | |||
Line 1: | Line 1: | ||
+ | ===<u>[[Process Group - Process Control Data#Etching .28Process Control Data.29|Process Control Data]]</u>=== |
||
− | {{Recipe Table Explanation}} |
||
+ | <small>''See [[Process Group - Process Control Data#Etching .28Process Control Data.29|linked page]] for [https://en.wikipedia.org/wiki/Statistical_process_control process control data] (dep rate/stress etc. over time), for a selection of often-used thin-film depositions.''</small> |
||
+ | |||
+ | ===Dry Etching Tools/Materials Table=== |
||
+ | |||
+ | *<small>'''R''': ''Recipe is available. Clicking this link will take you to the recipe.''</small> |
||
+ | *<small>'''A''': ''Material is available for use, but no recipes are provided.''</small> |
||
+ | |||
{| class="wikitable" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center; font-size: 95%" border="1" |
{| class="wikitable" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center; font-size: 95%" border="1" |
||
+ | |- |
||
+ | ! colspan="18" width="725" height="45" |<div style="font-size: 150%;">Dry Etching Recipes</div> |
||
|- bgcolor="#d0e7ff" |
|- bgcolor="#d0e7ff" |
||
+ | | bgcolor="#eaecf0" | <!-- INTENTIONALLY LEFT BLANK --> |
||
− | ! colspan="17" width="725" height="45" |<div style="font-size: 150%;">Dry Etching Recipes</div> |
||
+ | ! colspan="3" |'''[[RIE Etching Recipes|RIE Etching]]''' |
||
+ | ! colspan="6" |'''[[ICP Etching Recipes|ICP Etching]]''' |
||
+ | ! colspan="5" bgcolor="#d0e7ff" align="center" |'''[[Oxygen Plasma System Recipes|Oxygen Plasma Systems]]''' |
||
+ | ! colspan="3" bgcolor="#d0e7ff" align="center" |'''[[Other Dry Etching Recipes|Other Dry Etchers]]''' |
||
|- bgcolor="#d0e7ff" |
|- bgcolor="#d0e7ff" |
||
+ | ! bgcolor="#d0e7ff" align="center" |'''Material''' |
||
− | |<!-- INTENTIONALLY LEFT BLANK --> |
||
+ | | bgcolor="#daf1ff" |[[RIE_Etching_Recipes#RIE_2_.28MRC.29|RIE 2<br> <span style="font-size: 88%;">(MRC)</span>]] |
||
− | ! colspan="4" width="300" height="35" align="center" bgcolor="#d0e7ff" |'''[[RIE Etching Recipes|RIE Etching]]''' |
||
+ | | bgcolor="#daf1ff" |[[RIE_Etching_Recipes#RIE_3_.28MRC.29|RIE 3<br> <span style="font-size: 88%;">(MRC)</span>]] |
||
− | ! colspan="5" |'''[[ICP Etching Recipes|ICP Etching]]''' |
||
+ | | bgcolor="#daf1ff" |[[RIE_Etching_Recipes#RIE_5_.28PlasmaTherm.29|RIE 5<br><span style="font-size: 88%;">(PlasmaTherm)</span>]] |
||
− | ! colspan="4" align="center" bgcolor="#d0e7ff" |'''[[Oxygen Plasma System Recipes|Oxygen Plasma Systems]]''' |
||
+ | | bgcolor="#daf1ff" |[[ICP_Etching_Recipes#DSEIII_.28PlasmaTherm.2FDeep_Silicon_Etcher.29|DSEIII<br><span style="font-size: 88%;">(PlasmaTherm)</span>]] |
||
− | ! colspan="3" align="center" bgcolor="#d0e7ff" |'''[[Other Dry Etching Recipes|Other Dry Etchers]]''' |
||
+ | | bgcolor="#daf1ff" |[[ICP Etching Recipes#PlasmaTherm.2FSLR Fluorine Etcher|Fluorine ICP <span style="font-size: 88%;">(PlasmaTherm)</span>]] |
||
− | |- |
||
+ | | bgcolor="#daf1ff" |[[ICP_Etching_Recipes#ICP_Etch_1_.28Panasonic_E626I.29|ICP Etch 1<br><span style="font-size: 88%;">(Panasonic E626I)</span>]] |
||
− | ! width="65" align="center" bgcolor="#d0e7ff" |'''Material''' |
||
− | | |
+ | | bgcolor="#daf1ff" |[[ICP_Etching_Recipes#ICP_Etch_2_.28Panasonic_E640.29|ICP Etch 2<br><span style="font-size: 88%;">(Panasonic E640)</span>]] |
− | | |
+ | | bgcolor="#daf1ff" |[[ICP Etching Recipes#Oxford ICP Etcher .28PlasmaPro 100 Cobra.29|Oxford ICP <span style="font-size: 88%;">(PlasmaPro 100)</span>]] |
− | | |
+ | | bgcolor="#daf1ff" |[[ICP_Etching_Recipes#ICP-Etch_.28Unaxis_VLR.29|ICP-Etch<br><span style="font-size: 88%;">(Unaxis VLR)</span>]] |
− | | |
+ | | bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#Ashers_.28Technics_PEII.29|Ashers<br><span style="font-size: 88%;">(Technics PEII)</span>]] |
+ | | bgcolor="#daf1ff" | |
||
− | | width="100" bgcolor="#daf1ff" |[[ICP_Etching_Recipes#DSEIII_.28PlasmaTherm.2FDeep_Silicon_Etcher.29|DSEIII<br>(PlasmaTherm)]] |
||
+ | | bgcolor="#daf1ff" |[[Oxygen Plasma System Recipes#Plasma Clean .28YES EcoClean.29|Plasma Clean <span style="font-size: 88%;">(YES EcoClean)</span>]] |
||
− | | width="100" bgcolor="#daf1ff" |[https://www.nanotech.ucsb.edu/wiki/index.php/ICP_Etching_Recipes#PlasmaTherm.2FSLR_Fluorine_Etcher SLR Fluorine ICP (PlasmaTherm)] |
||
− | | |
+ | | bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#UV_Ozone_Reactor|UV Ozone Reactor]] |
− | | |
+ | | bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#Plasma_Activation_.28EVG_810.29|Plasma Activation<br><span style="font-size: 88%;">(EVG 810)</span>]] |
− | | |
+ | | bgcolor="#daf1ff" |[[Other_Dry_Etching_Recipes#XeF2_Etch_.28Xetch.29|XeF2 Etch<br><span style="font-size: 88%;">(Xetch)</span>]] |
− | | |
+ | | bgcolor="#daf1ff" |[[Other_Dry_Etching_Recipes#Vapor_HF_Etch_.28uETCH.29|Vapor HF Etch<br><span style="font-size: 88%;">(uETCH)</span>]] |
− | | |
+ | | bgcolor="#daf1ff" |[[Other_Dry_Etching_Recipes#CAIBE_.28Oxford_Ion_Mill.29|CAIBE<br><span style="font-size: 88%;">(Oxford)</span>]] |
− | | width="85" bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#UV_Ozone_Reactor|UV Ozone Reactor]] |
||
− | | width="85" bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#Plasma_Activation_.28EVG_810.29|Plasma Activation<br>(EVG 810)]] |
||
− | | width="85" bgcolor="#daf1ff" |[[Other_Dry_Etching_Recipes#XeF2_Etch_.28Xetch.29|XeF2 Etch<br>(Xetch)]] |
||
− | | width="85" bgcolor="#daf1ff" |[[Other_Dry_Etching_Recipes#Vapor_HF_Etch_.28uETCH.29|Vapor HF Etch<br>(uETCH)]] |
||
− | | width="85" bgcolor="#daf1ff" |[[Other_Dry_Etching_Recipes#CAIBE_.28Oxford_Ion_Mill.29|CAIBE<br>(Oxford)]] |
||
|- bgcolor="#eeffff" |
|- bgcolor="#eeffff" |
||
− | ! |
+ | ! bgcolor="#d0e7ff" align="center" |Ag |
| |
| |
||
| |
| |
||
Line 45: | Line 53: | ||
| |
| |
||
| |
| |
||
+ | |A |
||
− | |- bgcolor="#eeffff" |
||
− | + | |- bgcolor="#ffffff" |
|
+ | ! bgcolor="#d0e7ff" align="center" |Al |
||
− | | |
||
| |
| |
||
| |
| |
||
Line 63: | Line 71: | ||
| |
| |
||
| |
| |
||
+ | | |
||
+ | |A |
||
|- bgcolor="#eeffff" |
|- bgcolor="#eeffff" |
||
− | ! |
+ | ! bgcolor="#d0e7ff" align="center" |Au |
| |
| |
||
| |
| |
||
Line 80: | Line 90: | ||
| |
| |
||
| |
| |
||
− | |[https://www.nanotech.ucsb.edu/wiki/index.php/Other_Dry_Etching_Recipes#CAIBE_.28Oxford_Ion_Mill.29 A] |
||
− | |- bgcolor="#eeffff" |
||
− | ! align="center" bgcolor="#d0e7ff" |Cr |
||
| |
| |
||
+ | |{{rl|Other Dry Etching Recipes|Other Dry Etch (CAIBE (Oxford Ion Mill))}} |
||
+ | |- bgcolor="#ffffff" |
||
+ | ! bgcolor="#d0e7ff" align="center" |Cr |
||
| |
| |
||
| |
| |
||
Line 99: | Line 109: | ||
| |
| |
||
| |
| |
||
+ | | |
||
+ | |A |
||
|- bgcolor="#eeffff" |
|- bgcolor="#eeffff" |
||
− | ! |
+ | ! bgcolor="#d0e7ff" align="center" |Cu |
| |
| |
||
| |
| |
||
Line 117: | Line 129: | ||
| |
| |
||
| |
| |
||
− | | |
+ | |A |
− | + | |- bgcolor="#ffffff" |
|
+ | ! bgcolor="#d0e7ff" align="center" |Ge |
||
| |
| |
||
| |
| |
||
Line 124: | Line 137: | ||
| |
| |
||
| |
| |
||
+ | |A |
||
+ | |A |
||
| |
| |
||
| |
| |
||
Line 131: | Line 146: | ||
| |
| |
||
| |
| |
||
+ | |A |
||
| |
| |
||
|A |
|A |
||
− | | |
||
− | | |
||
|- bgcolor="#eeffff" |
|- bgcolor="#eeffff" |
||
− | ! |
+ | ! bgcolor="#d0e7ff" align="center" |Mo |
| |
| |
||
| |
| |
||
Line 153: | Line 167: | ||
| |
| |
||
| |
| |
||
+ | |A |
||
|- |
|- |
||
+ | !Nb |
||
− | ! align="center" bgcolor="#d0e7ff" |Ni |
||
| |
| |
||
| |
| |
||
Line 160: | Line 175: | ||
| |
| |
||
| |
| |
||
+ | |A |
||
+ | |A |
||
| |
| |
||
| |
| |
||
Line 170: | Line 187: | ||
| |
| |
||
| |
| |
||
+ | |- bgcolor="#ffffff" |
||
− | |{{rl|Other Dry Etching Recipes|Other Dry Etch (CAIBE (Oxford Ion Mill))}} |
||
+ | ! bgcolor="#d0e7ff" align="center" |Ni |
||
− | |- |
||
+ | | |
||
− | ! align="center" bgcolor="#d0e7ff" |Pt |
||
| |
| |
||
| |
| |
||
Line 190: | Line 207: | ||
|{{rl|Other Dry Etching Recipes|Other Dry Etch (CAIBE (Oxford Ion Mill))}} |
|{{rl|Other Dry Etching Recipes|Other Dry Etch (CAIBE (Oxford Ion Mill))}} |
||
|- |
|- |
||
+ | !Os |
||
− | ! align="center" bgcolor="#d0e7ff" |Ru |
||
− | | |
||
| |
| |
||
| |
| |
||
Line 198: | Line 214: | ||
| |
| |
||
|A |
|A |
||
+ | |A |
||
− | |{{Rl|ICP Etching Recipes|Ru (Ruthenium) Etch (Panasonic 2)}} |
||
+ | | |
||
+ | | |
||
| |
| |
||
| |
| |
||
Line 208: | Line 226: | ||
| |
| |
||
|- bgcolor="#eeffff" |
|- bgcolor="#eeffff" |
||
− | ! |
+ | ! bgcolor="#d0e7ff" align="center" |Pt |
| |
| |
||
| |
| |
||
| |
| |
||
| |
| |
||
− | |{{rl|ICP Etching Recipes|DSEIII_(PlasmaTherm/Deep_Silicon_Etcher)}} |
||
− | |{{Rl|ICP Etching Recipes|Si Etching}} |
||
| |
| |
||
| |
| |
||
Line 222: | Line 238: | ||
| |
| |
||
| |
| |
||
− | |{{rl|Other Dry Etching Recipes|Other Dry Etch (XeF2 Etcher)}} |
||
| |
| |
||
| |
| |
||
− | |- |
||
− | ! align="center" bgcolor="#d0e7ff" |Ta |
||
| |
| |
||
| |
| |
||
| |
| |
||
+ | |{{rl|Other Dry Etching Recipes|Other Dry Etch (CAIBE (Oxford Ion Mill))}} |
||
+ | |- bgcolor="#ffffff" |
||
+ | ! bgcolor="#d0e7ff" align="center" |Ru |
||
| |
| |
||
| |
| |
||
Line 235: | Line 251: | ||
| |
| |
||
| |
| |
||
+ | |A |
||
+ | |{{Rl|ICP Etching Recipes|Ru (Ruthenium) Etch (Panasonic 2)}} |
||
| |
| |
||
| |
| |
||
Line 243: | Line 261: | ||
| |
| |
||
| |
| |
||
− | |- |
||
− | ! align="center" bgcolor="#d0e7ff" |Ti |
||
| |
| |
||
+ | |A |
||
+ | |- bgcolor="#eeffff" |
||
+ | ! bgcolor="#d0e7ff" align="center" |Si |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | |{{rl|ICP Etching Recipes|DSEIII_(PlasmaTherm/Deep_Silicon_Etcher)}} |
||
+ | |{{Rl|ICP Etching Recipes|Si Etching}} |
||
+ | | |
||
+ | | |
||
+ | |A |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | |{{rl|Other Dry Etching Recipes|Other Dry Etch (XeF2 Etcher)}} |
||
+ | | |
||
+ | |A |
||
+ | |- bgcolor="#ffffff" |
||
+ | ! bgcolor="#d0e7ff" align="center" |Ta |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | |A |
||
+ | |A |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | |A |
||
+ | |- bgcolor="#eeffff" |
||
+ | ! bgcolor="#d0e7ff" align="center" |Ti |
||
| |
| |
||
| |
| |
||
Line 261: | Line 318: | ||
| |
| |
||
| |
| |
||
− | |- |
||
− | ! align="center" bgcolor="#d0e7ff" |Al<sub>2</sub>O<sub>3</sub> |
||
| |
| |
||
+ | |A |
||
+ | |- bgcolor="#ffffff" |
||
+ | ! bgcolor="#d0e7ff" align="center" |Al<sub>2</sub>O<sub>3</sub> |
||
| |
| |
||
| |
| |
||
Line 269: | Line 327: | ||
| |
| |
||
| |
| |
||
+ | |A |
||
+ | |[https://wiki.nanotech.ucsb.edu/w/index.php?title=ICP_Etching_Recipes#Al2O3_Etching_.28Panasonic_2.29 R] |
||
| |
| |
||
− | |[https://www.nanotech.ucsb.edu/wiki/index.php/ICP_Etching_Recipes#Al2O3_Etching_.28Panasonic_2.29 R] |
||
| |
| |
||
| |
| |
||
Line 279: | Line 338: | ||
| |
| |
||
| |
| |
||
+ | |A |
||
|- bgcolor="#eeffff" |
|- bgcolor="#eeffff" |
||
− | ! |
+ | ! bgcolor="#d0e7ff" align="center" |Al<sub>2</sub>O<sub>3 (Sapphire)</sub> |
− | | |
||
| |
| |
||
| |
| |
||
Line 297: | Line 356: | ||
| |
| |
||
| |
| |
||
− | |- |
||
− | ! align="center" bgcolor="#d0e7ff" |AlGaAs |
||
| |
| |
||
+ | |A |
||
+ | |- bgcolor="#ffffff" |
||
+ | ! bgcolor="#d0e7ff" align="center" |AlGaAs |
||
| |
| |
||
| |
| |
||
Line 307: | Line 367: | ||
|{{rl|ICP Etching Recipes|AlGaAs Etch (Panasonic 1)}} |
|{{rl|ICP Etching Recipes|AlGaAs Etch (Panasonic 1)}} |
||
| |
| |
||
+ | |[[ICP Etching Recipes#GaAs Etch .28Oxford ICP Etcher.29|R]] |
||
|{{rl|ICP Etching Recipes|ICP-Etch (Unaxis VLR)|GaAs-AlGaAs Etch (Unaxis VLR)|AlGaAs Etch (Unaxis VLR)}} |
|{{rl|ICP Etching Recipes|ICP-Etch (Unaxis VLR)|GaAs-AlGaAs Etch (Unaxis VLR)|AlGaAs Etch (Unaxis VLR)}} |
||
| |
| |
||
Line 315: | Line 376: | ||
| |
| |
||
| |
| |
||
+ | |A |
||
|- bgcolor="#eeffff" |
|- bgcolor="#eeffff" |
||
− | ! |
+ | ! bgcolor="#d0e7ff" align="center" |AlGaN |
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | |[[ICP Etching Recipes#GaN Etch .28Oxford ICP Etcher.29|R]] |
||
+ | |{{rl|ICP Etching Recipes|GaN Etch (Unaxis VLR)}} |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | |A |
||
+ | |- bgcolor="#ffffff" |
||
+ | ! bgcolor="#d0e7ff" align="center" |AlN |
||
| |
| |
||
| |
| |
||
Line 333: | Line 414: | ||
| |
| |
||
| |
| |
||
+ | |A |
||
|- |
|- |
||
+ | !BCB |
||
− | ! align="center" bgcolor="#d0e7ff" |AlN |
||
| |
| |
||
| |
| |
||
Line 340: | Line 422: | ||
| |
| |
||
| |
| |
||
+ | |A |
||
| |
| |
||
| |
| |
||
| |
| |
||
− | |{{rl|ICP Etching Recipes|GaN Etch (Unaxis VLR)}} |
||
| |
| |
||
| |
| |
||
Line 351: | Line 433: | ||
| |
| |
||
| |
| |
||
− | |- bgcolor="#eeffff" |
||
− | ! align="center" bgcolor="#d0e7ff" |CdZnTe |
||
| |
| |
||
+ | |- bgcolor="#eeffff" |
||
+ | ! bgcolor="#d0e7ff" align="center" |CdZnTe |
||
|{{rl|RIE Etching Recipes|CdZnTe Etch (RIE 2)}} |
|{{rl|RIE Etching Recipes|CdZnTe Etch (RIE 2)}} |
||
| |
| |
||
Line 369: | Line 451: | ||
| |
| |
||
| |
| |
||
− | |- bgcolor="#eeffff" |
||
− | ! align="center" bgcolor="#d0e7ff" |GaAs |
||
| |
| |
||
+ | |A |
||
+ | |- bgcolor="#ffffff" |
||
+ | ! bgcolor="#d0e7ff" align="center" |GaAs |
||
| |
| |
||
| |
| |
||
Line 379: | Line 462: | ||
|{{rl|ICP Etching Recipes|GaAs-AlGaAs_Etch_.28Panasonic_1.29}} |
|{{rl|ICP Etching Recipes|GaAs-AlGaAs_Etch_.28Panasonic_1.29}} |
||
|{{rl|ICP Etching Recipes|GaAs Etch (Panasonic 2)}} |
|{{rl|ICP Etching Recipes|GaAs Etch (Panasonic 2)}} |
||
+ | |[[ICP Etching Recipes#GaAs Etch .28Oxford ICP Etcher.29|R]] |
||
|{{rl|ICP Etching Recipes|ICP-Etch (Unaxis VLR)|GaAs-AlGaAs Etch (Unaxis VLR)|GaAs Etch (Unaxis VLR)}} |
|{{rl|ICP Etching Recipes|ICP-Etch (Unaxis VLR)|GaAs-AlGaAs Etch (Unaxis VLR)|GaAs Etch (Unaxis VLR)}} |
||
| |
| |
||
Line 387: | Line 471: | ||
| |
| |
||
| |
| |
||
− | | |
+ | |A |
− | + | |- bgcolor="#eeffff" |
|
+ | ! bgcolor="#d0e7ff" align="center" |GaN |
||
− | | |
||
| |
| |
||
| |
| |
||
Line 396: | Line 480: | ||
| |
| |
||
|{{rl|ICP Etching Recipes|GaN Etch (Panasonic 1)}} |
|{{rl|ICP Etching Recipes|GaN Etch (Panasonic 1)}} |
||
− | | |
+ | |A |
+ | |[[ICP Etching Recipes#GaN Etch .28Oxford ICP Etcher.29|R]] |
||
|{{rl|ICP Etching Recipes|GaN Etch (Unaxis VLR)}} |
|{{rl|ICP Etching Recipes|GaN Etch (Unaxis VLR)}} |
||
| |
| |
||
Line 405: | Line 490: | ||
| |
| |
||
| |
| |
||
+ | |A |
||
− | |- bgcolor="#eeffff" |
||
− | + | |- bgcolor="#ffffff" |
|
+ | ! bgcolor="#d0e7ff" align="center" |GaSb |
||
− | | |
||
− | | |
||
| |
| |
||
| |
| |
||
Line 414: | Line 498: | ||
| |
| |
||
| |
| |
||
+ | |A |
||
+ | |A |
||
|A |
|A |
||
|{{rl|ICP Etching Recipes|ICP-Etch (Unaxis VLR)|GaSb Etch Unaxis VLR)}} |
|{{rl|ICP Etching Recipes|ICP-Etch (Unaxis VLR)|GaSb Etch Unaxis VLR)}} |
||
Line 423: | Line 509: | ||
| |
| |
||
| |
| |
||
+ | |A |
||
|- bgcolor="#eeffff" |
|- bgcolor="#eeffff" |
||
− | ! |
+ | ! bgcolor="#d0e7ff" align="center" |HfO<sub>2</sub> |
| |
| |
||
| |
| |
||
Line 441: | Line 528: | ||
| |
| |
||
| |
| |
||
+ | |A |
||
− | |- bgcolor="#eeffff" |
||
− | + | |- bgcolor="#ffffff" |
|
+ | ! bgcolor="#d0e7ff" align="center" |InGaAlAs |
||
− | | |
||
|{{rl|RIE Etching Recipes|RIE 2 (MRC)|InP-InGaAsP-InGaAlAs Etching (RIE 2)|InP Etch (RIE 2)}} |
|{{rl|RIE Etching Recipes|RIE 2 (MRC)|InP-InGaAsP-InGaAlAs Etching (RIE 2)|InP Etch (RIE 2)}} |
||
| |
| |
||
Line 451: | Line 538: | ||
| |
| |
||
| |
| |
||
+ | |A |
||
|{{rl|ICP Etching Recipes|ICP-Etch (Unaxis VLR)|InP-InGaAs-InAlAs Etch (Unaxis VLR)|InP Etch (Unaxis VLR)}} |
|{{rl|ICP Etching Recipes|ICP-Etch (Unaxis VLR)|InP-InGaAs-InAlAs Etch (Unaxis VLR)|InP Etch (Unaxis VLR)}} |
||
| |
| |
||
Line 459: | Line 547: | ||
| |
| |
||
| |
| |
||
− | | |
+ | |A |
− | + | |- bgcolor="#eeffff" |
|
+ | ! bgcolor="#d0e7ff" align="center" |InGaAsP |
||
− | | |
||
|{{rl|RIE Etching Recipes|RIE 2 (MRC)|InP-InGaAsP-InGaAlAs Etching (RIE 2)|InP Etch (RIE 2)}} |
|{{rl|RIE Etching Recipes|RIE 2 (MRC)|InP-InGaAsP-InGaAlAs Etching (RIE 2)|InP Etch (RIE 2)}} |
||
| |
| |
||
Line 469: | Line 557: | ||
| |
| |
||
| |
| |
||
+ | |[[ICP Etching Recipes#InP Ridge Etch .28Oxford ICP Etcher.29|R]] |
||
|{{rl|ICP Etching Recipes|ICP-Etch (Unaxis VLR)|InP-InGaAs-InAlAs Etch (Unaxis VLR)|InP Etch (Unaxis VLR)}} |
|{{rl|ICP Etching Recipes|ICP-Etch (Unaxis VLR)|InP-InGaAs-InAlAs Etch (Unaxis VLR)|InP Etch (Unaxis VLR)}} |
||
| |
| |
||
Line 477: | Line 566: | ||
| |
| |
||
| |
| |
||
+ | |A |
||
− | |- bgcolor="#eeffff" |
||
− | + | |- bgcolor="#ffffff" |
|
+ | ! bgcolor="#d0e7ff" align="center" |InP |
||
− | | |
||
|{{rl|RIE Etching Recipes|RIE 2 (MRC)|InP-InGaAsP-InGaAlAs Etching (RIE 2)|InP Etch (RIE 2)}} |
|{{rl|RIE Etching Recipes|RIE 2 (MRC)|InP-InGaAsP-InGaAlAs Etching (RIE 2)|InP Etch (RIE 2)}} |
||
| |
| |
||
Line 487: | Line 576: | ||
|A |
|A |
||
|A |
|A |
||
+ | |[[ICP Etching Recipes#InP Ridge Etch .28Oxford ICP Etcher.29|R]] |
||
|{{rl|ICP Etching Recipes|ICP-Etch (Unaxis VLR)|InP-InGaAs-InAlAs Etch (Unaxis VLR)|InP Etch (Unaxis VLR)}} |
|{{rl|ICP Etching Recipes|ICP-Etch (Unaxis VLR)|InP-InGaAs-InAlAs Etch (Unaxis VLR)|InP Etch (Unaxis VLR)}} |
||
| |
| |
||
Line 495: | Line 585: | ||
| |
| |
||
| |
| |
||
+ | |{{rl|Other Dry Etching Recipes|Other Dry Etch (CAIBE (Oxford Ion Mill))}} |
||
+ | |- bgcolor="#eeffff" |
||
+ | ! bgcolor="#d0e7ff" align="center" |ITO |
||
+ | |{{rl|RIE Etching Recipes|ITO Etch (RIE 2)}} |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | |A |
||
|- |
|- |
||
+ | !LiNbO3 |
||
− | ! align="center" bgcolor="#d0e7ff" |ITO |
||
| |
| |
||
− | |{{rl|RIE Etching Recipes|ITO Etch (RIE 2)}} |
||
| |
| |
||
| |
| |
||
Line 513: | Line 622: | ||
| |
| |
||
| |
| |
||
+ | | |
||
− | |- bgcolor="#eeffff" |
||
+ | |A |
||
+ | |- bgcolor="#ffffff" |
||
!Photoresist |
!Photoresist |
||
& ARC |
& ARC |
||
+ | | |
||
+ | |A |
||
+ | |[https://wiki.nanotech.ucsb.edu/wiki/RIE_Etching_Recipes#Photoresist_and_ARC_.28RIE_5.29 R] |
||
+ | | |
||
+ | |[https://wiki.nanotech.ucsb.edu/wiki/ICP_Etching_Recipes#Photoresist_.26_ARC_.28Fluorine_ICP_Etcher.29 R] |
||
+ | |[https://wiki.nanotech.ucsb.edu/wiki/ICP_Etching_Recipes#Photoresist_and_ARC_Etching_.28Panasonic_1.29 R] |
||
+ | |[https://wiki.nanotech.ucsb.edu/wiki/ICP_Etching_Recipes#Photoresist_and_ARC_etching_.28Panasonic_2.29 R] |
||
+ | | |
||
+ | | |
||
+ | |R |
||
+ | | |
||
+ | |R |
||
+ | | |
||
+ | | |
||
| |
| |
||
| |
| |
||
|A |
|A |
||
+ | |- |
||
− | |[https://www.nanotech.ucsb.edu/wiki/index.php/RIE_Etching_Recipes#Photoresist_and_ARC R] |
||
+ | !Ru |
||
+ | | |
||
+ | | |
||
| |
| |
||
| |
| |
||
− | |[https://www.nanotech.ucsb.edu/wiki/index.php/ICP_Etching_Recipes#Photoresist_and_ARC_Etching R] |
||
− | |[https://www.nanotech.ucsb.edu/wiki/index.php/ICP_Etching_Recipes#Photoresist_and_ARC_etching_2 R] |
||
| |
| |
||
|A |
|A |
||
+ | |[[ICP Etching Recipes#Ru .28Ruthenium.29 Etch .28Panasonic 2.29|R]] |
||
− | |A |
||
| |
| |
||
| |
| |
||
Line 532: | Line 658: | ||
| |
| |
||
| |
| |
||
− | |- |
||
− | ! align="center" bgcolor="#d0e7ff" |SiC |
||
| |
| |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | |- bgcolor="#eeffff" |
||
+ | ! bgcolor="#d0e7ff" align="center" |SiC |
||
| |
| |
||
| |
| |
||
Line 550: | Line 680: | ||
| |
| |
||
| |
| |
||
− | |- |
||
− | ! align="center" bgcolor="#d0e7ff" |SiN |
||
| |
| |
||
+ | |A |
||
+ | |- bgcolor="#ffffff" |
||
+ | ! bgcolor="#d0e7ff" align="center" |SiN |
||
| |
| |
||
|{{rl|RIE Etching Recipes|RIE 3 (MRC)|SiN<sub>x</sub> Etching (RIE 3)}} |
|{{rl|RIE Etching Recipes|RIE 3 (MRC)|SiN<sub>x</sub> Etching (RIE 3)}} |
||
| |
| |
||
| |
| |
||
− | | |
+ | |A |
|{{rl|ICP Etching Recipes|SiNx Etching (Panasonic 1)}} |
|{{rl|ICP Etching Recipes|SiNx Etching (Panasonic 1)}} |
||
|{{rl|ICP Etching Recipes|SiNx Etching (Panasonic 2)}} |
|{{rl|ICP Etching Recipes|SiNx Etching (Panasonic 2)}} |
||
+ | | |
||
| |
| |
||
|A |
|A |
||
Line 568: | Line 700: | ||
| |
| |
||
| |
| |
||
+ | |A |
||
|- bgcolor="#eeffff" |
|- bgcolor="#eeffff" |
||
− | ! |
+ | ! bgcolor="#d0e7ff" align="center" |SiO<sub>2</sub> |
− | | |
||
| |
| |
||
|{{rl|RIE Etching Recipes|RIE 3 (MRC)|SiO<sub>2</sub> Etching (RIE 3)}} |
|{{rl|RIE Etching Recipes|RIE 3 (MRC)|SiO<sub>2</sub> Etching (RIE 3)}} |
||
| |
| |
||
| |
| |
||
+ | |{{rl|ICP Etching Recipes|SiO2 Etching (Fluorine ICP Etcher)}} |
||
− | |A |
||
|{{rl|ICP Etching Recipes|SiO2 Etching (Panasonic 1)}} |
|{{rl|ICP Etching Recipes|SiO2 Etching (Panasonic 1)}} |
||
|{{rl|ICP Etching Recipes|SiO2 Etching (Panasonic 2)}} |
|{{rl|ICP Etching Recipes|SiO2 Etching (Panasonic 2)}} |
||
Line 584: | Line 716: | ||
| |
| |
||
| |
| |
||
− | |{{rl|Other Dry Etching Recipes|Other Dry Etch (Vapor HF Etcher)}} |
||
| |
| |
||
− | |- bgcolor="#eeffff" |
||
− | ! align="center" bgcolor="#d0e7ff" |SiOxNy |
||
| |
| |
||
+ | |{{rl|Other Dry Etching Recipes|Other Dry Etch (Vapor HF Etcher)}} |
||
+ | |A |
||
+ | |- bgcolor="#ffffff" |
||
+ | ! bgcolor="#d0e7ff" align="center" |SiOxNy |
||
| |
| |
||
| |
| |
||
Line 604: | Line 737: | ||
| |
| |
||
| |
| |
||
+ | | |
||
+ | |A |
||
|- |
|- |
||
+ | !SU8 |
||
− | ! align="center" bgcolor="#d0e7ff" |Ta<sub>2</sub>O<sub>5</sub> |
||
| |
| |
||
| |
| |
||
Line 611: | Line 746: | ||
| |
| |
||
| |
| |
||
+ | |A |
||
| |
| |
||
| |
| |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | |- bgcolor="#eeffff" |
||
+ | ! bgcolor="#d0e7ff" align="center" |Ta<sub>2</sub>O<sub>5</sub> |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | |A |
||
|[https://www.osapublishing.org/optica/abstract.cfm?uri=optica-4-5-532 A] |
|[https://www.osapublishing.org/optica/abstract.cfm?uri=optica-4-5-532 A] |
||
| |
| |
||
Line 622: | Line 775: | ||
| |
| |
||
| |
| |
||
− | |- |
||
− | ! align="center" bgcolor="#d0e7ff" |TiN |
||
| |
| |
||
+ | |A |
||
+ | |- bgcolor="#ffffff" |
||
+ | ! bgcolor="#d0e7ff" align="center" |TiN |
||
| |
| |
||
| |
| |
||
Line 640: | Line 794: | ||
| |
| |
||
| |
| |
||
+ | | |
||
+ | |A |
||
|- bgcolor="#eeffff" |
|- bgcolor="#eeffff" |
||
− | ! |
+ | ! bgcolor="#d0e7ff" align="center" |TiO<sub>2</sub> |
| |
| |
||
| |
| |
||
Line 658: | Line 814: | ||
| |
| |
||
| |
| |
||
+ | |A |
||
− | |- bgcolor="#eeffff" |
||
− | + | |- bgcolor="#ffffff" |
|
+ | ! bgcolor="#d0e7ff" align="center" |W-TiW |
||
− | | |
||
| |
| |
||
| |
| |
||
Line 676: | Line 832: | ||
| |
| |
||
| |
| |
||
+ | | |
||
+ | |A |
||
|- bgcolor="#eeffff" |
|- bgcolor="#eeffff" |
||
− | ! |
+ | ! bgcolor="#d0e7ff" align="center" |ZnO<sub>2</sub> |
| |
| |
||
| |
| |
||
Line 694: | Line 852: | ||
| |
| |
||
| |
| |
||
− | | |
+ | |A |
− | + | |- bgcolor="#ffffff" |
|
+ | ! bgcolor="#d0e7ff" align="center" |ZnS |
||
− | | |
||
|{{rl|RIE Etching Recipes|ZnS Etching (RIE 2)}} |
|{{rl|RIE Etching Recipes|ZnS Etching (RIE 2)}} |
||
| |
| |
||
Line 712: | Line 870: | ||
| |
| |
||
| |
| |
||
− | |- |
||
− | ! align="center" bgcolor="#d0e7ff" |ZnSe |
||
| |
| |
||
+ | |A |
||
+ | |- bgcolor="#eeffff" |
||
+ | ! bgcolor="#d0e7ff" align="center" |ZnSe |
||
|{{rl|RIE Etching Recipes|ZnS Etching (RIE 2)}} |
|{{rl|RIE Etching Recipes|ZnS Etching (RIE 2)}} |
||
| |
| |
||
Line 730: | Line 889: | ||
| |
| |
||
| |
| |
||
− | |- |
||
− | ! align="center" bgcolor="#d0e7ff" |ZrO<sub>2</sub> |
||
| |
| |
||
+ | |A |
||
+ | |- bgcolor="#ffffff" |
||
+ | ! bgcolor="#d0e7ff" align="center" |ZrO<sub>2</sub> |
||
| |
| |
||
| |
| |
||
Line 748: | Line 908: | ||
| |
| |
||
| |
| |
||
− | | |
+ | | |
+ | |A |
||
− | ! align="center" bgcolor="#d0e7ff" |'''Material''' |
||
− | | bgcolor="# |
+ | |- bgcolor="#eeffff" |
+ | ! bgcolor="#d0e7ff" align="center" |'''Material''' |
||
− | | bgcolor="#daf1ff" |[[RIE_Etching_Recipes#RIE_2_.28MRC.29|RIE 2<br> (MRC)]] |
||
− | | bgcolor="#daf1ff" |[[RIE_Etching_Recipes# |
+ | | bgcolor="#daf1ff" |[[RIE_Etching_Recipes#RIE_2_.28MRC.29|RIE 2<br> <span style="font-size: 88%;">(MRC)</span>]] |
− | | bgcolor="#daf1ff" |[[RIE_Etching_Recipes# |
+ | | bgcolor="#daf1ff" |[[RIE_Etching_Recipes#RIE_3_.28MRC.29|RIE 3<br> <span style="font-size: 88%;">(MRC)</span>]] |
− | | bgcolor="#daf1ff" |[[ |
+ | | bgcolor="#daf1ff" |[[RIE_Etching_Recipes#RIE_5_.28PlasmaTherm.29|RIE 5<br><span style="font-size: 88%;">(PlasmaTherm)</span>]] |
− | | bgcolor="#daf1ff" |[[ |
+ | | bgcolor="#daf1ff" |[[ICP_Etching_Recipes#DSEIII_.28PlasmaTherm.2FDeep_Silicon_Etcher.29|DSEIII<br><span style="font-size: 88%;">(PlasmaTherm)</span>]] |
− | | bgcolor="#daf1ff" |[[ |
+ | | bgcolor="#daf1ff" |[[ICP Etching Recipes#PlasmaTherm.2FSLR Fluorine Etcher|Fluorine ICP <span style="font-size: 88%;">(PlasmaTherm)</span>]] |
− | | bgcolor="#daf1ff" |[[ICP_Etching_Recipes# |
+ | | bgcolor="#daf1ff" |[[ICP_Etching_Recipes#ICP_Etch_1_.28Panasonic_E626I.29|ICP Etch 1<br><span style="font-size: 88%;">(Panasonic E626I)</span>]] |
− | | bgcolor="#daf1ff" |[[ICP_Etching_Recipes# |
+ | | bgcolor="#daf1ff" |[[ICP_Etching_Recipes#ICP_Etch_2_.28Panasonic_E640.29|ICP Etch 2<br><span style="font-size: 88%;">(Panasonic E640)</span>]] |
− | | bgcolor="#daf1ff" |[[ |
+ | | bgcolor="#daf1ff" |[[ICP Etching Recipes#Oxford ICP Etcher .28PlasmaPro 100 Cobra.29|Oxford ICP <span style="font-size: 88%;">(PlasmaPro 100)</span>]] |
− | | bgcolor="#daf1ff" |[[ |
+ | | bgcolor="#daf1ff" |[[ICP_Etching_Recipes#ICP-Etch_.28Unaxis_VLR.29|ICP-Etch<br><span style="font-size: 88%;">(Unaxis VLR)</span>]] |
+ | | bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#Ashers_.28Technics_PEII.29|Ashers<br><span style="font-size: 88%;">(Technics PEII)</span>]] |
||
+ | | |
||
+ | | bgcolor="#daf1ff" |[[Oxygen Plasma System Recipes#Plasma Clean .28YES EcoClean.29|Plasma Clean <span style="font-size: 88%;">(YES EcoClean)</span>]] |
||
| bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#UV_Ozone_Reactor|UV Ozone Reactor]] |
| bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#UV_Ozone_Reactor|UV Ozone Reactor]] |
||
− | | bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#Plasma_Activation_.28EVG_810.29|Plasma Activation<br>(EVG 810)]] |
+ | | bgcolor="#daf1ff" |[[Oxygen_Plasma_System_Recipes#Plasma_Activation_.28EVG_810.29|Plasma Activation<br><span style="font-size: 88%;">(EVG 810)</span>]] |
− | | bgcolor="#daf1ff" |[[Other_Dry_Etching_Recipes#XeF2_Etch_.28Xetch.29|XeF2 Etch<br>(Xetch)]] |
+ | | bgcolor="#daf1ff" |[[Other_Dry_Etching_Recipes#XeF2_Etch_.28Xetch.29|XeF2 Etch<br><span style="font-size: 88%;">(Xetch)</span>]] |
− | | bgcolor="#daf1ff" |[[Other_Dry_Etching_Recipes#Vapor_HF_Etch_.28uETCH.29|Vapor HF Etch<br>(uETCH)]] |
+ | | bgcolor="#daf1ff" |[[Other_Dry_Etching_Recipes#Vapor_HF_Etch_.28uETCH.29|Vapor HF Etch<br><span style="font-size: 88%;">(uETCH)</span>]] |
− | | bgcolor="#daf1ff" |[[Other_Dry_Etching_Recipes#CAIBE_.28Oxford_Ion_Mill.29|CAIBE<br>(Oxford)]] |
+ | | bgcolor="#daf1ff" |[[Other_Dry_Etching_Recipes#CAIBE_.28Oxford_Ion_Mill.29|CAIBE<br><span style="font-size: 88%;">(Oxford)</span>]] |
|} |
|} |
||
Revision as of 16:54, 29 September 2022
Process Control Data
See linked page for process control data (dep rate/stress etc. over time), for a selection of often-used thin-film depositions.
Dry Etching Tools/Materials Table
- R: Recipe is available. Clicking this link will take you to the recipe.
- A: Material is available for use, but no recipes are provided.