Difference between revisions of "Dry Etching Recipes"
Jump to navigation
Jump to search
Line 7: | Line 7: | ||
! width="300" bgcolor="#D0E7FF" align="center" colspan="5" | '''[[ICP Etching Recipes|ICP Etching]]''' |
! width="300" bgcolor="#D0E7FF" align="center" colspan="5" | '''[[ICP Etching Recipes|ICP Etching]]''' |
||
|- |
|- |
||
− | !width=" |
+ | !width="65" bgcolor="#D0E7FF" align="center" | '''Material''' |
|width="65" bgcolor="#DAF1FF" | [[RIE 1 (Custom)|RIE 1<br>(Custom)]] |
|width="65" bgcolor="#DAF1FF" | [[RIE 1 (Custom)|RIE 1<br>(Custom)]] |
||
|width="65" bgcolor="#DAF1FF" | [[RIE 2 (MRC)|RIE 2<br> (MRC)]] |
|width="65" bgcolor="#DAF1FF" | [[RIE 2 (MRC)|RIE 2<br> (MRC)]] |
||
Line 17: | Line 17: | ||
|width="85" bgcolor="#DAF1FF" | [[ICP-Etch (Unaxis VLR)|ICP-Etch<br>(Unaxis VLR)]] |
|width="85" bgcolor="#DAF1FF" | [[ICP-Etch (Unaxis VLR)|ICP-Etch<br>(Unaxis VLR)]] |
||
|- |
|- |
||
− | ! |
+ | ! bgcolor="#D0E7FF" align="center" | Al |
| |
| |
||
| |
| |
||
Line 27: | Line 27: | ||
| |
| |
||
|- |
|- |
||
− | ! |
+ | ! bgcolor="#D0E7FF" align="center" | Ti |
| |
| |
||
| |
| |
||
Line 37: | Line 37: | ||
| |
| |
||
|- |
|- |
||
− | ! |
+ | ! bgcolor="#D0E7FF" align="center" | Cr |
| |
| |
||
| |
| |
||
Line 47: | Line 47: | ||
| |
| |
||
|- |
|- |
||
− | ! |
+ | ! bgcolor="#D0E7FF" align="center" | Ge |
| |
| |
||
| |
| |
||
Line 57: | Line 57: | ||
| |
| |
||
|- |
|- |
||
− | ! |
+ | ! bgcolor="#D0E7FF" align="center" | Ag |
| |
| |
||
| |
| |
||
Line 67: | Line 67: | ||
| |
| |
||
|- |
|- |
||
− | ! |
+ | ! bgcolor="#D0E7FF" align="center" | Ru |
| |
| |
||
| |
| |
||
Line 77: | Line 77: | ||
| |
| |
||
|- |
|- |
||
− | ! |
+ | ! bgcolor="#D0E7FF" align="center" | Mo |
| |
| |
||
| |
| |
||
Line 87: | Line 87: | ||
| |
| |
||
|- |
|- |
||
− | ! |
+ | ! bgcolor="#D0E7FF" align="center" | Ta |
| |
| |
||
| |
| |
||
Line 97: | Line 97: | ||
| |
| |
||
|- |
|- |
||
− | ! |
+ | ! bgcolor="#D0E7FF" align="center" | W |
| |
| |
||
| |
| |
||
Line 107: | Line 107: | ||
| |
| |
||
|- |
|- |
||
− | ! |
+ | ! bgcolor="#D0E7FF" align="center" | Al<sub>2</sub>O<sub>3</sub> |
| |
| |
||
| |
| |
||
Line 117: | Line 117: | ||
| |
| |
||
|- |
|- |
||
− | ! |
+ | ! bgcolor="#D0E7FF" align="center" | HfO<sub>2</sub> |
| |
| |
||
| |
| |
||
Line 127: | Line 127: | ||
| |
| |
||
|- |
|- |
||
− | ! |
+ | ! bgcolor="#D0E7FF" align="center" | ITo |
| |
| |
||
| |
| |
||
Line 137: | Line 137: | ||
| |
| |
||
|- |
|- |
||
− | ! |
+ | ! bgcolor="#D0E7FF" align="center" | SiO<sub>2</sub> |
| |
| |
||
| |
| |
||
Line 147: | Line 147: | ||
| |
| |
||
|- |
|- |
||
− | ! |
+ | ! bgcolor="#D0E7FF" align="center" | SiN |
| |
| |
||
| |
| |
||
Line 157: | Line 157: | ||
| |
| |
||
|- |
|- |
||
− | ! |
+ | ! bgcolor="#D0E7FF" align="center" | SiOxNy |
| |
| |
||
| |
| |
||
Line 167: | Line 167: | ||
| |
| |
||
|- |
|- |
||
− | ! |
+ | ! bgcolor="#D0E7FF" align="center" | Ta<sub>2</sub>O<sub>5</sub> |
| |
| |
||
| |
| |
||
Line 177: | Line 177: | ||
| |
| |
||
|- |
|- |
||
− | ! |
+ | ! bgcolor="#D0E7FF" align="center" | TiO<sub>2</sub> |
| |
| |
||
| |
| |
||
Line 187: | Line 187: | ||
| |
| |
||
|- |
|- |
||
− | ! |
+ | ! bgcolor="#D0E7FF" align="center" | TiN |
| |
| |
||
| |
| |
||
Line 197: | Line 197: | ||
| |
| |
||
|- |
|- |
||
− | ! |
+ | ! bgcolor="#D0E7FF" align="center" | ZnO<sub>2</sub> |
| |
| |
||
| |
| |
||
Line 207: | Line 207: | ||
| |
| |
||
|- |
|- |
||
− | ! |
+ | ! bgcolor="#D0E7FF" align="center" | ZrO<sub>2</sub> |
| |
| |
||
| |
| |
||
Line 217: | Line 217: | ||
| |
| |
||
|- |
|- |
||
− | ! |
+ | ! bgcolor="#D0E7FF" align="center" | GaAs |
| |
| |
||
| |
| |
||
Line 227: | Line 227: | ||
| |
| |
||
|- |
|- |
||
− | ! |
+ | ! bgcolor="#D0E7FF" align="center" | AlGaAs |
| |
| |
||
| |
| |
||
Line 237: | Line 237: | ||
| |
| |
||
|- |
|- |
||
− | ! |
+ | ! bgcolor="#D0E7FF" align="center" | InGaAlAs |
| |
| |
||
| |
| |
||
Line 247: | Line 247: | ||
| |
| |
||
|- |
|- |
||
− | ! |
+ | ! bgcolor="#D0E7FF" align="center" | InGaAsP |
| |
| |
||
| |
| |
||
Line 257: | Line 257: | ||
| |
| |
||
|- |
|- |
||
− | ! |
+ | ! bgcolor="#D0E7FF" align="center" | InP |
| |
| |
||
| |
| |
||
Line 267: | Line 267: | ||
| |
| |
||
|- |
|- |
||
− | ! |
+ | ! bgcolor="#D0E7FF" align="center" | GaN |
| |
| |
||
| |
| |
||
Line 277: | Line 277: | ||
| |
| |
||
|- |
|- |
||
− | ! |
+ | ! bgcolor="#D0E7FF" align="center" | AlGaN |
| |
| |
||
| |
| |
||
Line 287: | Line 287: | ||
| |
| |
||
|- |
|- |
||
− | ! |
+ | ! bgcolor="#D0E7FF" align="center" | AlN |
| |
| |
||
| |
| |
||
Line 297: | Line 297: | ||
| |
| |
||
|- |
|- |
||
− | ! |
+ | ! bgcolor="#D0E7FF" align="center" | GaN |
| |
| |
||
| |
| |
||
Line 307: | Line 307: | ||
| |
| |
||
|- |
|- |
||
− | ! |
+ | ! bgcolor="#D0E7FF" align="center" | AlGaN |
| |
| |
||
| |
| |
||
Line 317: | Line 317: | ||
| |
| |
||
|- |
|- |
||
− | ! |
+ | ! bgcolor="#D0E7FF" align="center" | AlN |
| |
| |
||
| |
| |
||
Line 327: | Line 327: | ||
| |
| |
||
|- |
|- |
||
− | ! |
+ | ! bgcolor="#D0E7FF" align="center" | GaSb |
| |
| |
||
| |
| |
||
Line 337: | Line 337: | ||
| |
| |
||
|- |
|- |
||
− | ! |
+ | ! bgcolor="#D0E7FF" align="center" | CdTe |
| |
| |
||
| |
| |
||
Line 347: | Line 347: | ||
| |
| |
||
|- |
|- |
||
− | ! |
+ | ! bgcolor="#D0E7FF" align="center" | ZnSe |
| |
| |
||
| |
| |
||
Line 357: | Line 357: | ||
| |
| |
||
|- |
|- |
||
− | ! |
+ | ! bgcolor="#D0E7FF" align="center" | Si |
| |
| |
||
| |
| |
||
Line 367: | Line 367: | ||
| |
| |
||
|- |
|- |
||
− | ! |
+ | ! bgcolor="#D0E7FF" align="center" | SiC |
| |
| |
||
| |
| |
||
Line 377: | Line 377: | ||
| |
| |
||
|- |
|- |
||
− | ! |
+ | ! bgcolor="#D0E7FF" align="center" | Sapphire |
| |
| |
||
| |
| |
||
Line 387: | Line 387: | ||
| |
| |
||
|} |
|} |
||
− | |||
− | = Recipes = |
||
− | |||
− | == RIE Etching == |
||
− | |||
− | == ICP Etching == |
Revision as of 13:45, 18 July 2012
Dry Etching Recipes
| |||||||||
---|---|---|---|---|---|---|---|---|---|
RIE Etching | ICP Etching | ||||||||
Material | RIE 1 (Custom) |
RIE 2 (MRC) |
RIE 3 (MRC) |
RIE 5 (PlasmaTherm) |
Si Deep RIE (PlasmaTherm/Bosch Etch) |
ICP Etch 1 (Panasonic E626I) |
ICP Etch 2 (Panasonic E640) |
ICP-Etch (Unaxis VLR) | |
Al | |||||||||
Ti | |||||||||
Cr | |||||||||
Ge | |||||||||
Ag | |||||||||
Ru | |||||||||
Mo | |||||||||
Ta | |||||||||
W | |||||||||
Al2O3 | |||||||||
HfO2 | |||||||||
ITo | |||||||||
SiO2 | |||||||||
SiN | |||||||||
SiOxNy | |||||||||
Ta2O5 | |||||||||
TiO2 | |||||||||
TiN | |||||||||
ZnO2 | |||||||||
ZrO2 | |||||||||
GaAs | |||||||||
AlGaAs | |||||||||
InGaAlAs | |||||||||
InGaAsP | |||||||||
InP | |||||||||
GaN | |||||||||
AlGaN | |||||||||
AlN | |||||||||
GaN | |||||||||
AlGaN | |||||||||
AlN | |||||||||
GaSb | |||||||||
CdTe | |||||||||
ZnSe | |||||||||
Si | |||||||||
SiC | |||||||||
Sapphire |