Difference between revisions of "ASML DUV: Edge Bead Removal via Photolithography"
Jump to navigation
Jump to search
(note on I-line process) |
|||
(One intermediate revision by the same user not shown) | |||
Line 1: | Line 1: | ||
− | The metal edge-bead removal masks are in the Suss MA-6 Contact Aligner drawers, and I recommend the "4mm recessed" |
+ | The metal edge-bead removal masks are in the Suss MA-6 Contact Aligner drawers, and I recommend the "4mm recessed". |
It loses a bit more device area, but significantly lowers the risk of breaking a wafer in clamped systems such as the DSEiii. |
It loses a bit more device area, but significantly lowers the risk of breaking a wafer in clamped systems such as the DSEiii. |
||
− | (This process can easily be transferred to I-Line photoresists, using the [[Contact Aligner (SUSS MA-6)|Suss MA-6]] for flood exposure.) |
+ | (This process can easily be transferred to I-Line photoresists, using the [[Contact Aligner (SUSS MA-6)|Suss MA-6]] for flood exposure instead of DUV Flood expose.) |
− | === |
+ | ===Photo-EBR Process=== |
+ | |||
− | * |
+ | *Spun/cure a DUV photoresist using your standard photolith. params (for example [[Stepper Recipes#Positive Resist .28ASML DUV.29|UV6]]). |
− | * |
+ | *Place the wafer on the [[DUV Flood Expose|'''DUV Flood Exposer''']] with the metal mask in place. |
− | * |
+ | *Turn on rotation on slow (so mask doesn't move), lamp warmup is not required. |
− | * |
+ | *Expose for 13 sec, with slow rotation. |
− | * |
+ | *''Optionally:'' PEB 135°C, 60sec, Develop, dry (in SRD), then proceed. This did not affect my primary lithography when I did this step separately. I've also done photo-EBR where I combined this EBR exposure with the primary Imaging litho. and only did a single develop. |
− | * |
+ | *Load wafer into ASML & Expose your process |
− | * |
+ | *PEB 135°C, 90sec |
− | * |
+ | *300MiF develop as per your normal process. |
− | ** |
+ | **(If you did not develop the EBR yet, it should go away in this step.) |
+ | |||
+ | Demis D. John, 2018-10-22 |
Latest revision as of 23:06, 4 October 2022
The metal edge-bead removal masks are in the Suss MA-6 Contact Aligner drawers, and I recommend the "4mm recessed".
It loses a bit more device area, but significantly lowers the risk of breaking a wafer in clamped systems such as the DSEiii.
(This process can easily be transferred to I-Line photoresists, using the Suss MA-6 for flood exposure instead of DUV Flood expose.)
Photo-EBR Process
- Spun/cure a DUV photoresist using your standard photolith. params (for example UV6).
- Place the wafer on the DUV Flood Exposer with the metal mask in place.
- Turn on rotation on slow (so mask doesn't move), lamp warmup is not required.
- Expose for 13 sec, with slow rotation.
- Optionally: PEB 135°C, 60sec, Develop, dry (in SRD), then proceed. This did not affect my primary lithography when I did this step separately. I've also done photo-EBR where I combined this EBR exposure with the primary Imaging litho. and only did a single develop.
- Load wafer into ASML & Expose your process
- PEB 135°C, 90sec
- 300MiF develop as per your normal process.
- (If you did not develop the EBR yet, it should go away in this step.)