Difference between revisions of "Wet Etching Recipes"
(link to Chemicals List) |
m (KOH: added mention of "low-stress" SiN) |
||
Line 26: | Line 26: | ||
Please add any confirmed etches from this reference to the {{HLink|Wet Etching Recipes|The Master Table of Wet Etching (Include All Materials)}}. |
Please add any confirmed etches from this reference to the {{HLink|Wet Etching Recipes|The Master Table of Wet Etching (Include All Materials)}}. |
||
− | |||
− | ==Dielectric etching== |
||
==Organic removal== |
==Organic removal== |
||
+ | * Piranha Solution. '''Careful!''' Read about how to prepare and handle this safely: |
||
+ | ** [http://web.mit.edu/cortiz/www/PiranhaSafety.doc MIT's Piranha Solution safety document] |
||
+ | ** [https://www.ehs.harvard.edu/sites/default/files/lab_safety_guideline_piranha_etch.pdf Harvard EHS's Handling Document] |
||
==Gold Plating== |
==Gold Plating== |
||
− | ==Chemi-Mechanical Polishing (CMP)== |
+ | ==[[Chemical-Mechanical Polisher (Logitech)|Chemi-Mechanical Polishing (CMP)]]== |
− | |||
− | |||
− | ==Example Wet Etching Table== |
||
− | How to use the Master Table of Wet Etching: |
||
+ | == [[Mechanical Polisher (Allied)|Mechanical Polishing (Allied)]] == |
||
⚫ | |||
+ | ==Adding a new entry to the Table== |
||
+ | When entering a new etch into the table: |
||
+ | * Make a row for every etchant used in the solution such that the information can be sorted by etchant. For example, the InP etch HCl:H3PO4(1:3) and H3PO4:HCl(3:1). |
||
⚫ | |||
This multiple entry method may seem laborious for the person entering a new etch, however the power of sorting by selective materials and chemicals in a table with all materials is great. |
This multiple entry method may seem laborious for the person entering a new etch, however the power of sorting by selective materials and chemicals in a table with all materials is great. |
||
Line 238: | Line 239: | ||
|~730 |
|~730 |
||
|High, Crystallographic |
|High, Crystallographic |
||
− | |Si3N4 - |
+ | |Low-Stress Si3N4 - either [[PECVD Recipes#Low-Stress SiN deposition .28PECVD .232.29|PECVD #2]] or Commercial LPCVD Si3N4 |
+ | Other Si3N4 also OK. |
||
|High |
|High |
||
|Measured In-House |
|Measured In-House |
Revision as of 23:31, 29 June 2021
See the Master Wet Etching Table at the bottom of this page for wet-etch rates in various experiments we have tested.
Chemicals Available
- The Chemical Lists show stocked chemicals, photolithography chemicals, and how to bring new chemicals.
References
- Etch rates for Micromachining Processing (IEEE Jnl. MEMS, 1996) - includes tables of etch rates of numerous metals vs. various wet and dry etchants.
- Etch rates for micromachining-Part II (IEEE Jnl. MEMS, 2003) - expanded tables containing resists, dielectrics, metals and semiconductors vs. many wet etch chemicals.
- Guide to references on III±V semiconductor chemical etching - exhaustive list of wet etchants for etching various semiconductors, including selective etches.
- Transene's Chemical Compatibility Chart provides a useful quick-reference for which Transene etchants attack which materials.
- As a side-note, Transene provides many pre-mixed solutions that you can order, saving you the time and uncertainty of measuring/mixing such chemicals yourself. Make sure you check with us before ordering so we know how to handle the chemical before it arrives.
Compound Semiconductor Etching
Guide to references on III±V semiconductor chemical etching
Please add any confirmed etches from this reference to the The Master Table of Wet Etching (Include All Materials).
Metal Etching
- Selective Wet Etch of Cr over Ta using Cr Etchant
- Wet Etch of ITO using Heated, Diluted HCl Solution
Silicon etching
Etch rates for micromachining processing
Etch rates for micromachining processing-part II
Please add any confirmed etches from this reference to the The Master Table of Wet Etching (Include All Materials).
Organic removal
- Piranha Solution. Careful! Read about how to prepare and handle this safely:
Gold Plating
Chemi-Mechanical Polishing (CMP)
Mechanical Polishing (Allied)
Adding a new entry to the Table
When entering a new etch into the table:
- Make a row for every etchant used in the solution such that the information can be sorted by etchant. For example, the InP etch HCl:H3PO4(1:3) and H3PO4:HCl(3:1).
- Likewise, if etch is known to be selective to multiple materials the etch should have a row for each material. For example HCl:H3PO4(1:3) is selective to both InGaAs and InGaAsP.
This multiple entry method may seem laborious for the person entering a new etch, however the power of sorting by selective materials and chemicals in a table with all materials is great.
Material | Etchant | Rate (nm/min) | Anisotropy | Selective to | Selectivity | Ref. | Notes | Confirmed by | Extra column |
---|---|---|---|---|---|---|---|---|---|
InP | HCl:H3PO4(1:3) | ~1000 | Highly | InGaAs | High | Lamponi (p.102) | Example | Jon Doe | Example |
InP | HCl:H3PO4(1:3) | ~1000 | Highly | InGaAsP | High | Lamponi (p.102) | Example | Jon Doe | Example |
InP | H3PO4:HCl(3:1) | ~1000 | Highly | InGaAs | High | Lamponi (p.102) | Example | Jon Doe | Example |
InP | H3PO4:HCl(3:1) | ~1000 | Highly | InGaAsP | High | Lamponi (p.102) | Example | Jon Doe | Example |
The Master Table of Wet Etching (Include All Materials)
Use the ↑ ↓ Arrows in the header row to sort the entire table by material, selectivity, etchant etc.
Material | Etchant | Rate (nm/min) | Anisotropy | Selective to | Selectivity | Ref. | Notes | Confirmed by | Extra Notes |
---|---|---|---|---|---|---|---|---|---|
InP | HCl:H3PO4 (1:3) | ~1000 | Highly | InGaAs | High | Lamponi (p.102) | Example | Jon Doe | Example |
InP | HCl:H3PO4 (1:3) | ~1000 | Highly | InGaAsP | High | Lamponi (p.102) | Example | Jon Doe | Example |
InP | H3PO4:HCl (3:1) | ~1000 | Highly | InGaAs | High | Lamponi (p.102) | Example | Jon Doe | Example |
InP | H3PO4:HCl (3:1) | ~1000 | Highly | InGaAsP | High | Lamponi (p.102) | Example | Jon Doe | Example |
Al2O3 (ALD Plasma 300C) | Developer: 300MIF | ~1.6 | None | Most non-Al Materials. | High | Measured in-house | Rate slows with time. | JTB | Example |
Al2O3 (ALD Plasma 300C) | Developer: 400K | ~2.2 | None | Most non-Al Materials. | High | Measured in-house | Rate slows with time. | JTB | Example |
Al2O3 (ALD Plasma 300C) | Developer: 400K (1:4) | ~1.6 | None | Most non-Al Materials. | High | Measured in-house | Rate slows with time. | JTB | Example |
Al2O3 (ALD Plasma 300C) | NH4OH:H2O2:H2O (1:2:50) | ~<0.5 | Measured in-house | Rate slows with time | JTB | Example | |||
Al2O3 (IBD) | HF ("Buffered HF Improved", Transene) | ~170 | None | Photoresist | High | Measured in-house | May need to increase adhesion with thin SiO2 layer, and 100°C baked HMDS. | Biljana Stamenic | 2017-12 |
Al2O3 (IBD) | Developer: 726 MiF | 3.5 | None | Most non-Al Materials. | Measured in-house | Demis D. John | 2017-11 | ||
Al2O3 (AJA#4) | Developer: 300 MiF | 4.30 | None | Most non-Al Materials. | Measured in-house | Demis D. John | 2018-02 | ||
SiO2 (PECVD #1) | HF ("Buffered HF Improved", Transene) | ~500 | None | Photoresist | High | Measured in-house | May need to increase adhesion with 100°C baked HMDS. | Biljana Stamenic | 2017 |
SiO2 (PECVD #2) | HF ("Buffered HF Improved", Transene) | ~500 | None | Photoresist | High | Measured in-house | May need to increase adhesion with 100°C baked HMDS. | Biljana Stamenic | 2017 |
SiO2 (IBD) | HF ("Buffered HF Improved", Transene) | ~350 | None | Photoresist | High | Measured in-house | Biljana Stamenic | 2016 | |
Si3N4 (PECVD#1) | HF ("Buffered HF Improved", Transene) | 85 | None | Photoresist | High | Measured in-house | Biljana Stamenic | 2018-04 | |
Si3N4 (PECVD#2) | HF ("Buffered HF Improved", Transene) | 35–45 | None | Photoresist | High | Measured in-house | Biljana Stamenic | 2018-05 | |
Si3N4 Low-Stress (PECVD#2) | HF ("Buffered HF Improved", Transene) | 35–50 | None | Photoresist | High | Measured in-house | Biljana Stamenic | 2018-05 | |
Si3N4 (IBD) | HF ("Buffered HF Improved", Transene) | 5–15 | None | Photoresist | High | Measured in-house | Biljana Stamenic | 2014 | |
Ta2O5 (IBD) | HF ("Buffered HF Improved", Transene) | 0.4 | None | Photoresist | High | Measured in-house | Biljana Stamenic | 2016-12 | |
TiO2 (IBD) | HF ("Buffered HF Improved", Transene) | 1.0–2.0 | None | Photoresist | High | Measured in-house | Biljana Stamenic | 2014-12 | |
Si (<100> crystalline) | KOH (45%) @ 87°C | ~730 | High, Crystallographic | Low-Stress Si3N4 - either PECVD #2 or Commercial LPCVD Si3N4
Other Si3N4 also OK. |
High | Measured In-House | Use Covered, Heated vertical bath (Bay 4). Slight Bubbler. | Brian Thibeault | 2017 |