https://wiki.nanofab.ucsb.edu/w/index.php?title=Unaxis_wafer_coating_procedure&diff=158353&oldid=prev
John d: typos in units (nm/µm/mm), minor formatting
2020-08-13T04:29:25Z
<p>typos in units (nm/µm/mm), minor formatting</p>
<a href="https://wiki.nanofab.ucsb.edu/w/index.php?title=Unaxis_wafer_coating_procedure&diff=158353&oldid=158273">Show changes</a>
John d
https://wiki.nanofab.ucsb.edu/w/index.php?title=Unaxis_wafer_coating_procedure&diff=158273&oldid=prev
John d: link to recipes page
2020-07-16T07:20:47Z
<p>link to recipes page</p>
<table class="diff diff-contentalign-left diff-editfont-monospace" data-mw="interface">
<col class="diff-marker" />
<col class="diff-content" />
<col class="diff-marker" />
<col class="diff-content" />
<tr class="diff-title" lang="en">
<td colspan="2" style="background-color: #fff; color: #202122; text-align: center;">← Older revision</td>
<td colspan="2" style="background-color: #fff; color: #202122; text-align: center;">Revision as of 07:20, 16 July 2020</td>
</tr><tr>
<td colspan="2" class="diff-lineno">Line 1:</td>
<td colspan="2" class="diff-lineno">Line 1:</td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>=== Important Notes ===</div></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>=== Important Notes ===</div></td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>* Maximum 0.5µm of deposition prior to chamber cleaning, in order to maintain low particle counts.</div></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>* Maximum 0.5µm of deposition prior to chamber cleaning, in order to maintain low particle counts.</div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>* See the [[PECVD Recipes#ICP-PECVD .28Unaxis VLR.29|'''ICP-PECVD Unaxis Recipes''' page]] for thin-film properties of each of the following recipes.</div></td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>* We highly recommend using the [[Surface Analysis (KLA/Tencor Surfscan)|Surfscan particle counter]] to monitor particle counts on look-ahead wafers prior to deposition.</div></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>* We highly recommend using the [[Surface Analysis (KLA/Tencor Surfscan)|Surfscan particle counter]] to monitor particle counts on look-ahead wafers prior to deposition.</div></td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>** If you note abnormally high particle counts (>200), run chamber clean/season and retry. If particle counts are still high, notify the [[ICP-PECVD (Unaxis VLR)|tool supervisor]].</div></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>** If you note abnormally high particle counts (>200), run chamber clean/season and retry. If particle counts are still high, notify the [[ICP-PECVD (Unaxis VLR)|tool supervisor]].</div></td>
</tr>
<tr>
<td colspan="2" class="diff-lineno">Line 6:</td>
<td colspan="2" class="diff-lineno">Line 7:</td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>* For new recipes (as of Dec. 2019), users may '''only edit <u>Deposition Time</u>''', no other recipe modifications or customizations are permitted without staff approval.</div></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>* For new recipes (as of Dec. 2019), users may '''only edit <u>Deposition Time</u>''', no other recipe modifications or customizations are permitted without staff approval.</div></td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
</tr>
<tr>
<td class="diff-marker">−</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #ffe49c; vertical-align: top; white-space: pre-wrap;"><div>=== Unaxis SiO2 <del class="diffchange diffchange-inline">LDR</del> @250C deposition ===</div></td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>=== Unaxis SiO2 <ins class="diffchange diffchange-inline">Low Dep. Rate</ins> @250C deposition ===</div></td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>a) Prepare wafers:</div></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>a) Prepare wafers:</div></td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
</tr>
<tr>
<td colspan="2" class="diff-lineno">Line 33:</td>
<td colspan="2" class="diff-lineno">Line 34:</td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>e) Unload wafers when all runs are finished.</div></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>e) Unload wafers when all runs are finished.</div></td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
</tr>
<tr>
<td class="diff-marker">−</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #ffe49c; vertical-align: top; white-space: pre-wrap;"><div>=== Unaxis SiO2 <del class="diffchange diffchange-inline">HDR</del> <del class="diffchange diffchange-inline">@</del>250°C deposition ===</div></td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>=== Unaxis SiO2 <ins class="diffchange diffchange-inline">High Dep Rate</ins> 250°C deposition ===</div></td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>a) Prepare wafers:</div></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>a) Prepare wafers:</div></td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
</tr>
<tr>
<td colspan="2" class="diff-lineno">Line 60:</td>
<td colspan="2" class="diff-lineno">Line 61:</td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>e) Unload wafers when all runs are finished.</div></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>e) Unload wafers when all runs are finished.</div></td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
</tr>
<tr>
<td class="diff-marker">−</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #ffe49c; vertical-align: top; white-space: pre-wrap;"><div>=== Unaxis SiN <del class="diffchange diffchange-inline">@</del>250°C deposition ===</div></td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>=== Unaxis SiN 250°C deposition ===</div></td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>a) Prepare wafers:</div></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>a) Prepare wafers:</div></td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
</tr>
<tr>
<td colspan="2" class="diff-lineno">Line 85:</td>
<td colspan="2" class="diff-lineno">Line 86:</td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>e) Unload wafers when all runs are finished.</div></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>e) Unload wafers when all runs are finished.</div></td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
</tr>
<tr>
<td class="diff-marker">−</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #ffe49c; vertical-align: top; white-space: pre-wrap;"><div>=== Unaxis SiN <del class="diffchange diffchange-inline">LS</del> <del class="diffchange diffchange-inline">@</del>250°C deposition ===</div></td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>=== Unaxis SiN <ins class="diffchange diffchange-inline">Low-Stress</ins> 250°C deposition ===</div></td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>a) Prepare wafers:</div></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>a) Prepare wafers:</div></td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
</tr>
</table>
John d
https://wiki.nanofab.ucsb.edu/w/index.php?title=Unaxis_wafer_coating_procedure&diff=158272&oldid=prev
John d: /* Unaxis SiN LS @250°C deposition */ unbold
2020-07-16T07:18:34Z
<p><span dir="auto"><span class="autocomment">Unaxis SiN LS @250°C deposition: </span> unbold</span></p>
<table class="diff diff-contentalign-left diff-editfont-monospace" data-mw="interface">
<col class="diff-marker" />
<col class="diff-content" />
<col class="diff-marker" />
<col class="diff-content" />
<tr class="diff-title" lang="en">
<td colspan="2" style="background-color: #fff; color: #202122; text-align: center;">← Older revision</td>
<td colspan="2" style="background-color: #fff; color: #202122; text-align: center;">Revision as of 07:18, 16 July 2020</td>
</tr><tr>
<td colspan="2" class="diff-lineno">Line 85:</td>
<td colspan="2" class="diff-lineno">Line 85:</td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>e) Unload wafers when all runs are finished.</div></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>e) Unload wafers when all runs are finished.</div></td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
</tr>
<tr>
<td class="diff-marker">−</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #ffe49c; vertical-align: top; white-space: pre-wrap;"><div>=== <del class="diffchange diffchange-inline">'''</del>Unaxis SiN LS @250°C<del class="diffchange diffchange-inline">'''</del> <del class="diffchange diffchange-inline">'''</del>deposition<del class="diffchange diffchange-inline">'''</del> ===</div></td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>=== Unaxis SiN LS @250°C deposition ===</div></td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>a) Prepare wafers:</div></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>a) Prepare wafers:</div></td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
</tr>
</table>
John d
https://wiki.nanofab.ucsb.edu/w/index.php?title=Unaxis_wafer_coating_procedure&diff=158271&oldid=prev
John d: only edit dep. time
2020-07-16T07:17:17Z
<p>only edit dep. time</p>
<table class="diff diff-contentalign-left diff-editfont-monospace" data-mw="interface">
<col class="diff-marker" />
<col class="diff-content" />
<col class="diff-marker" />
<col class="diff-content" />
<tr class="diff-title" lang="en">
<td colspan="2" style="background-color: #fff; color: #202122; text-align: center;">← Older revision</td>
<td colspan="2" style="background-color: #fff; color: #202122; text-align: center;">Revision as of 07:17, 16 July 2020</td>
</tr><tr>
<td colspan="2" class="diff-lineno">Line 3:</td>
<td colspan="2" class="diff-lineno">Line 3:</td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>* We highly recommend using the [[Surface Analysis (KLA/Tencor Surfscan)|Surfscan particle counter]] to monitor particle counts on look-ahead wafers prior to deposition.</div></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>* We highly recommend using the [[Surface Analysis (KLA/Tencor Surfscan)|Surfscan particle counter]] to monitor particle counts on look-ahead wafers prior to deposition.</div></td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>** If you note abnormally high particle counts (>200), run chamber clean/season and retry. If particle counts are still high, notify the [[ICP-PECVD (Unaxis VLR)|tool supervisor]].</div></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>** If you note abnormally high particle counts (>200), run chamber clean/season and retry. If particle counts are still high, notify the [[ICP-PECVD (Unaxis VLR)|tool supervisor]].</div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>** You must measure particle count wafers '''before''' and after the deposition. See the procedures on the [[Surface Analysis (KLA/Tencor Surfscan)|Surfscan page]].</div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>* For new recipes (as of Dec. 2019), users may '''only edit <u>Deposition Time</u>''', no other recipe modifications or customizations are permitted without staff approval.</div></td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
</tr>
<tr>
<td class="diff-marker">−</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #ffe49c; vertical-align: top; white-space: pre-wrap;"><div>===<del class="diffchange diffchange-inline"> '''1.</del> Unaxis SiO2 LDR @250C deposition<del class="diffchange diffchange-inline">'''</del> ===</div></td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>=== Unaxis SiO2 LDR @250C deposition ===</div></td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>a) Prepare wafers:</div></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>a) Prepare wafers:</div></td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
</tr>
<tr>
<td colspan="2" class="diff-lineno">Line 31:</td>
<td colspan="2" class="diff-lineno">Line 33:</td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>e) Unload wafers when all runs are finished.</div></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>e) Unload wafers when all runs are finished.</div></td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
</tr>
<tr>
<td class="diff-marker">−</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #ffe49c; vertical-align: top; white-space: pre-wrap;"><div>===<del class="diffchange diffchange-inline"> '''2.</del> Unaxis SiO2 HDR @250°C deposition<del class="diffchange diffchange-inline">'''</del> ===</div></td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>=== Unaxis SiO2 HDR @250°C deposition ===</div></td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>a) Prepare wafers:</div></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>a) Prepare wafers:</div></td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
</tr>
<tr>
<td colspan="2" class="diff-lineno">Line 58:</td>
<td colspan="2" class="diff-lineno">Line 60:</td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>e) Unload wafers when all runs are finished.</div></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>e) Unload wafers when all runs are finished.</div></td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
</tr>
<tr>
<td class="diff-marker">−</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #ffe49c; vertical-align: top; white-space: pre-wrap;"><div>===<del class="diffchange diffchange-inline"> '''3.</del> Unaxis SiN @250°C deposition<del class="diffchange diffchange-inline">'''</del> ===</div></td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>=== Unaxis SiN @250°C deposition ===</div></td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>a) Prepare wafers:</div></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>a) Prepare wafers:</div></td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
</tr>
<tr>
<td colspan="2" class="diff-lineno">Line 83:</td>
<td colspan="2" class="diff-lineno">Line 85:</td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>e) Unload wafers when all runs are finished.</div></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>e) Unload wafers when all runs are finished.</div></td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
</tr>
<tr>
<td class="diff-marker">−</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #ffe49c; vertical-align: top; white-space: pre-wrap;"><div>===<del class="diffchange diffchange-inline"> 4.</del> '''Unaxis SiN LS @250°C''' '''deposition''' ===</div></td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>=== '''Unaxis SiN LS @250°C''' '''deposition''' ===</div></td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>a) Prepare wafers:</div></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>a) Prepare wafers:</div></td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
</tr>
</table>
John d
https://wiki.nanofab.ucsb.edu/w/index.php?title=Unaxis_wafer_coating_procedure&diff=158270&oldid=prev
John d: notes about 0.5µm max. dep, and particle counting
2020-07-16T07:13:16Z
<p>notes about 0.5µm max. dep, and particle counting</p>
<table class="diff diff-contentalign-left diff-editfont-monospace" data-mw="interface">
<col class="diff-marker" />
<col class="diff-content" />
<col class="diff-marker" />
<col class="diff-content" />
<tr class="diff-title" lang="en">
<td colspan="2" style="background-color: #fff; color: #202122; text-align: center;">← Older revision</td>
<td colspan="2" style="background-color: #fff; color: #202122; text-align: center;">Revision as of 07:13, 16 July 2020</td>
</tr><tr>
<td colspan="2" class="diff-lineno">Line 1:</td>
<td colspan="2" class="diff-lineno">Line 1:</td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>=== Important Notes ===</div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>* Maximum 0.5µm of deposition prior to chamber cleaning, in order to maintain low particle counts.</div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>* We highly recommend using the [[Surface Analysis (KLA/Tencor Surfscan)|Surfscan particle counter]] to monitor particle counts on look-ahead wafers prior to deposition.</div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>** If you note abnormally high particle counts (>200), run chamber clean/season and retry. If particle counts are still high, notify the [[ICP-PECVD (Unaxis VLR)|tool supervisor]].</div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"></td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>=== '''1. Unaxis SiO2 LDR @250C deposition''' ===</div></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>=== '''1. Unaxis SiO2 LDR @250C deposition''' ===</div></td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>a) Prepare wafers:</div></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>a) Prepare wafers:</div></td>
</tr>
</table>
John d
https://wiki.nanofab.ucsb.edu/w/index.php?title=Unaxis_wafer_coating_procedure&diff=158229&oldid=prev
Biljana: /* a) Prepare wafers: */
2020-07-02T19:03:26Z
<p><span dir="auto"><span class="autocomment">a) Prepare wafers:</span></span></p>
<table class="diff diff-contentalign-left diff-editfont-monospace" data-mw="interface">
<col class="diff-marker" />
<col class="diff-content" />
<col class="diff-marker" />
<col class="diff-content" />
<tr class="diff-title" lang="en">
<td colspan="2" style="background-color: #fff; color: #202122; text-align: center;">← Older revision</td>
<td colspan="2" style="background-color: #fff; color: #202122; text-align: center;">Revision as of 19:03, 2 July 2020</td>
</tr><tr>
<td colspan="2" class="diff-lineno">Line 79:</td>
<td colspan="2" class="diff-lineno">Line 79:</td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>=== 4. '''Unaxis SiN LS @250°C''' '''deposition''' ===</div></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>=== 4. '''Unaxis SiN LS @250°C''' '''deposition''' ===</div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker"><a class="mw-diff-movedpara-right" title="Paragraph was moved. Click to jump to old location." href="#movedpara_3_0_lhs">⚫</a></td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div><a name="movedpara_1_0_rhs"></a>a) Prepare wafers:</div></td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
</tr>
<tr>
<td class="diff-marker"><a class="mw-diff-movedpara-left" title="Paragraph was moved. Click to jump to new location." href="#movedpara_1_0_rhs">⚫</a></td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #ffe49c; vertical-align: top; white-space: pre-wrap;"><div><a name="movedpara_3_0_lhs"></a><del class="diffchange diffchange-inline">=== </del>a) Prepare wafers:<del class="diffchange diffchange-inline"> ===</del></div></td>
<td colspan="2" class="diff-empty"> </td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>· Regular 4 " Si wafer ~500nm think for seasoning </div></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>· Regular 4 " Si wafer ~500nm think for seasoning </div></td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
</tr>
</table>
Biljana
https://wiki.nanofab.ucsb.edu/w/index.php?title=Unaxis_wafer_coating_procedure&diff=158228&oldid=prev
Biljana: /* 1. Unaxis deposition - 300nm of SiO2 LDR film @250°C */
2020-07-02T19:02:52Z
<p><span dir="auto"><span class="autocomment">1. Unaxis deposition - 300nm of SiO2 LDR film @250°C</span></span></p>
<table class="diff diff-contentalign-left diff-editfont-monospace" data-mw="interface">
<col class="diff-marker" />
<col class="diff-content" />
<col class="diff-marker" />
<col class="diff-content" />
<tr class="diff-title" lang="en">
<td colspan="2" style="background-color: #fff; color: #202122; text-align: center;">← Older revision</td>
<td colspan="2" style="background-color: #fff; color: #202122; text-align: center;">Revision as of 19:02, 2 July 2020</td>
</tr><tr>
<td colspan="2" class="diff-lineno">Line 1:</td>
<td colspan="2" class="diff-lineno">Line 1:</td>
</tr>
<tr>
<td class="diff-marker">−</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #ffe49c; vertical-align: top; white-space: pre-wrap;"><div>=== '''1. Unaxis<del class="diffchange diffchange-inline"> deposition - 300nm of </del> SiO2 LDR <del class="diffchange diffchange-inline">film</del> <del class="diffchange diffchange-inline">@250°C</del>''' ===</div></td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>=== '''1. Unaxis SiO2 LDR <ins class="diffchange diffchange-inline">@250C</ins> <ins class="diffchange diffchange-inline">deposition</ins>''' ===</div></td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>a) Prepare wafers:</div></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>a) Prepare wafers:</div></td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
</tr>
</table>
Biljana
https://wiki.nanofab.ucsb.edu/w/index.php?title=Unaxis_wafer_coating_procedure&diff=158227&oldid=prev
Biljana at 19:01, 2 July 2020
2020-07-02T19:01:48Z
<p></p>
<table class="diff diff-contentalign-left diff-editfont-monospace" data-mw="interface">
<col class="diff-marker" />
<col class="diff-content" />
<col class="diff-marker" />
<col class="diff-content" />
<tr class="diff-title" lang="en">
<td colspan="2" style="background-color: #fff; color: #202122; text-align: center;">← Older revision</td>
<td colspan="2" style="background-color: #fff; color: #202122; text-align: center;">Revision as of 19:01, 2 July 2020</td>
</tr><tr>
<td colspan="2" class="diff-lineno">Line 26:</td>
<td colspan="2" class="diff-lineno">Line 26:</td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>e) Unload wafers when all runs are finished.</div></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>e) Unload wafers when all runs are finished.</div></td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
</tr>
<tr>
<td class="diff-marker">−</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #ffe49c; vertical-align: top; white-space: pre-wrap;"><div>'''2. Unaxis SiO2 HDR @250°C deposition'''</div></td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div><ins class="diffchange diffchange-inline">=== </ins>'''2. Unaxis SiO2 HDR @250°C deposition'''<ins class="diffchange diffchange-inline"> ===</ins></div></td>
</tr>
<tr>
<td class="diff-marker">−</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #ffe49c; vertical-align: top; white-space: pre-wrap;"></td>
<td colspan="2" class="diff-empty"> </td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>a) Prepare wafers:</div></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>a) Prepare wafers:</div></td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
</tr>
<tr>
<td colspan="2" class="diff-lineno">Line 54:</td>
<td colspan="2" class="diff-lineno">Line 53:</td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>e) Unload wafers when all runs are finished.</div></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>e) Unload wafers when all runs are finished.</div></td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
</tr>
<tr>
<td class="diff-marker">−</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #ffe49c; vertical-align: top; white-space: pre-wrap;"><div>'''3. Unaxis SiN @250°C deposition'''</div></td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div><ins class="diffchange diffchange-inline">=== </ins>'''3. Unaxis SiN @250°C deposition'''<ins class="diffchange diffchange-inline"> ===</ins></div></td>
</tr>
<tr>
<td class="diff-marker">−</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #ffe49c; vertical-align: top; white-space: pre-wrap;"></td>
<td colspan="2" class="diff-empty"> </td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>a) Prepare wafers:</div></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>a) Prepare wafers:</div></td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
</tr>
<tr>
<td colspan="2" class="diff-lineno">Line 80:</td>
<td colspan="2" class="diff-lineno">Line 78:</td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>e) Unload wafers when all runs are finished.</div></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>e) Unload wafers when all runs are finished.</div></td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
</tr>
<tr>
<td class="diff-marker">−</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #ffe49c; vertical-align: top; white-space: pre-wrap;"><div>4. '''Unaxis SiN LS @250°C''' '''deposition'''</div></td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div><ins class="diffchange diffchange-inline">=== </ins>4. '''Unaxis SiN LS @250°C''' '''deposition'''<ins class="diffchange diffchange-inline"> ===</ins></div></td>
</tr>
<tr>
<td class="diff-marker">−</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #ffe49c; vertical-align: top; white-space: pre-wrap;"></td>
<td colspan="2" class="diff-empty"> </td>
</tr>
<tr>
<td class="diff-marker"><a class="mw-diff-movedpara-left" title="Paragraph was moved. Click to jump to new location." href="#movedpara_10_0_rhs">⚫</a></td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #ffe49c; vertical-align: top; white-space: pre-wrap;"><div><a name="movedpara_8_1_lhs"></a>a) Prepare wafers:</div></td>
<td colspan="2" class="diff-empty"> </td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker"><a class="mw-diff-movedpara-right" title="Paragraph was moved. Click to jump to old location." href="#movedpara_8_1_lhs">⚫</a></td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div><a name="movedpara_10_0_rhs"></a><ins class="diffchange diffchange-inline">=== </ins>a) Prepare wafers:<ins class="diffchange diffchange-inline"> ===</ins></div></td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>· Regular 4 " Si wafer ~500nm think for seasoning </div></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>· Regular 4 " Si wafer ~500nm think for seasoning </div></td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
</tr>
</table>
Biljana
https://wiki.nanofab.ucsb.edu/w/index.php?title=Unaxis_wafer_coating_procedure&diff=158226&oldid=prev
Biljana at 19:01, 2 July 2020
2020-07-02T19:01:19Z
<p></p>
<table class="diff diff-contentalign-left diff-editfont-monospace" data-mw="interface">
<col class="diff-marker" />
<col class="diff-content" />
<col class="diff-marker" />
<col class="diff-content" />
<tr class="diff-title" lang="en">
<td colspan="2" style="background-color: #fff; color: #202122; text-align: center;">← Older revision</td>
<td colspan="2" style="background-color: #fff; color: #202122; text-align: center;">Revision as of 19:01, 2 July 2020</td>
</tr><tr>
<td colspan="2" class="diff-lineno">Line 1:</td>
<td colspan="2" class="diff-lineno">Line 1:</td>
</tr>
<tr>
<td class="diff-marker">−</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #ffe49c; vertical-align: top; white-space: pre-wrap;"><div>'''1. Unaxis deposition - 300nm of SiO2 LDR film @250°C'''</div></td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div><ins class="diffchange diffchange-inline">=== </ins>'''1. Unaxis deposition - 300nm of SiO2 LDR film @250°C'''<ins class="diffchange diffchange-inline"> ===</ins></div></td>
</tr>
<tr>
<td class="diff-marker">−</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #ffe49c; vertical-align: top; white-space: pre-wrap;"></td>
<td colspan="2" class="diff-empty"> </td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>a) Prepare wafers:</div></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>a) Prepare wafers:</div></td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
</tr>
</table>
Biljana
https://wiki.nanofab.ucsb.edu/w/index.php?title=Unaxis_wafer_coating_procedure&diff=158225&oldid=prev
Biljana: Created page with "'''1. Unaxis deposition - 300nm of SiO2 LDR film @250°C''' a) Prepare wafers: · Regular 4 " Si wafer ~500nm think for seasoning · Your substrate for d..."
2020-07-02T19:00:41Z
<p>Created page with "'''1. Unaxis deposition - 300nm of SiO2 LDR film @250°C''' a) Prepare wafers: · Regular 4 " Si wafer ~500nm think for seasoning · Your substrate for d..."</p>
<p><b>New page</b></p><div>'''1. Unaxis deposition - 300nm of SiO2 LDR film @250°C'''<br />
<br />
a) Prepare wafers:<br />
<br />
· Regular 4 " Si wafer ~500nm think for seasoning <br />
<br />
· Your substrate for deposition (if smaller then 4" needs to be loaded on a carrier)<br />
<br />
· Thick 4" Si wafer~(0.8-1um) for cleaning<br />
<br />
b) Load all 3 wafers in a cassette, making sure major flat is facing outside (toward you). Try to align flats for all three wafers.<br />
<br />
c) Edit '''standard recipes''' (for seasoning, deposition, and cleaning). You can '''ONLY change the time''' in these recipes.<br />
<br />
Seasoning recipe name: '''SiO2 seasoning''', '''t=2min'''<br />
<br />
Deposition recipe name: '''SiO2 LDR 250°C, t=780 sec'''<br />
<br />
Cleaning recipe name: '''Post dep PD''', '''t=900sec'''<br />
<br />
d) Run the job (first run seasoning, then deposition on your substate and cleaning at the end.<br />
<br />
You should monitor process at the very beginning to make sure there are no any issues with the run.<br />
<br />
· There is '''only one SiO2 seasoning recipe''' that is used for both LDR and HDR depositions. The goal in this step is to prepare the chamber and deposit ~200nm of SiO2 on walls.<br />
<br />
e) Unload wafers when all runs are finished.<br />
<br />
'''2. Unaxis SiO2 HDR @250°C deposition'''<br />
<br />
a) Prepare wafers:<br />
<br />
· Regular 4 " Si wafer ~500nm think for seasoning <br />
<br />
· Your substrate for deposition (if smaller then 4" needs to be loaded on a carrier)<br />
<br />
· Thick 4" Si wafer~(0.8-1um) for cleaning<br />
<br />
b) Load all wafers in a cassette, making sure major flat is facing outside (toward you). Try to align flats for all three wafers.<br />
<br />
c) Edit '''standard recipes''' (for seasoning, deposition, and cleaning). You can '''ONLY change the time''' in the recipe.<br />
<br />
Seasoning recipe name: '''SiO2 seasoning, t=2min'''<br />
<br />
Deposition recipe name: '''SiO2 HDR 250°C''', '''t=180 sec'''<br />
<br />
Cleaning recipe name: '''Post dep PD''', '''t=900sec'''<br />
<br />
d) Run the job (first run seasoning, then deposition on your substate and cleaning at the end.<br />
<br />
You should monitor process at the very beginning to make sure there are no any issues with the run.<br />
<br />
· There is '''only one SiO2 seasoning recipe''' that is used for both LDR and HDR depositions. The goal in this step is to prepare the chamber and deposit ~200nm of SiO2 on walls.<br />
<br />
e) Unload wafers when all runs are finished.<br />
<br />
'''3. Unaxis SiN @250°C deposition'''<br />
<br />
a) Prepare wafers:<br />
<br />
· Regular 4 " Si wafer ~500nm think for seasoning <br />
<br />
· Your substrate for deposition (if smaller then 4" needs to be loaded on a carrier)<br />
<br />
· Thick 4" Si wafer~(0.8-1um) for cleaning<br />
<br />
b) Load all wafers in a cassette, making sure major flat is facing outside (toward you). Try to align flats for all three wafers.<br />
<br />
c) Edit '''standard recipes''' (for seasoning, deposition, and cleaning). You can '''ONLY change the time''' in the recipe.<br />
<br />
Seasoning recipe name: '''SiN seasoning''', '''t=5min'''<br />
<br />
Deposition recipe name: '''SiN 250°C, t=480 sec'''<br />
<br />
Cleaning recipe name: '''Post dep PD,''' '''t=1500sec'''<br />
<br />
d) Run the job (first run seasoning, then deposition on your substate and cleaning at the end.<br />
<br />
You should monitor process at the very beginning to make sure there are no any issues with the run.<br />
<br />
e) Unload wafers when all runs are finished.<br />
<br />
4. '''Unaxis SiN LS @250°C''' '''deposition'''<br />
<br />
a) Prepare wafers:<br />
<br />
· Regular 4 " Si wafer ~500nm think for seasoning <br />
<br />
· Your substrate for deposition (if smaller then 4" needs to be loaded on a carrier)<br />
<br />
· Thick 4" Si wafer~(0.8-1um) for cleaning<br />
<br />
b) Load all wafers in a cassette, making sure major flat is facing outside (toward you). Try to align flats for all three wafers.<br />
<br />
c) Edit '''standard recipes''' (for seasoning, deposition, and cleaning). You can '''ONLY change the time''' in the recipe.<br />
<br />
Seasoning recipe name: '''SiN seasoning''', '''t=2min'''<br />
<br />
Deposition recipe name: '''SiN LS''' '''250°C''', '''t=180 sec'''<br />
<br />
Cleaning recipe name: '''Post dep PD,''' '''t=1500sec'''<br />
<br />
d) Run the job (first run seasoning, then deposition on your substate and cleaning at the end.<br />
<br />
You should monitor process at the very beginning to make sure there are no any issues with the run.<br />
<br />
e) Unload wafers when all runs are finished.</div>
Biljana