Data - InP Ridge Etch (Unaxis VLR)

PECVD SiO2 hardmask, patterned on Stepper #2 (AutoStep 200) & Panasonic ICP #1

InP Ridge Etch: 200°C, 1.4mT, 800W/125W, Cl2=6.3, H2=12.7, Ar=2.0 sccm, time=1min30sec (90sec)

Sample Size: 1x1cm epi-grade InP, ~30-40% SiO2 masking (NingC's pattern). Silicon carrier, no adhesive.

Conditioning: Prior to the etch, do O2 clean 15 minutes, then, chamber coating with the same recipe on 1/4-2" InP on Silicon carrier for 15 minutes.

Date Sample# Etch Rate (nm/min) Etch Selectivity (InP/SiO2) Comments SEM Images
4/28/22 NP_Unaxis_03 1.51 22.2 [1] [2]
3/30/22 NP_Unaxis_02 1.41 14.6 [1] [2]
3/9/22 NP_Unaxis_01 1.30 15.3 [1] [2]
11/8/2021 InP#2102 1.24 13.8 [1][2]
2/3/2021 InP#2101 1.30 16 [3][4]
8/30/2020 InP#2001 1.11 10.4 [5]
1/31/2019 InP#1901 0.88 9.7 [6][7]
12/10/2018 InP#1809 1.01 11.4 [8]
10/3/2018 InP#1808 1.01 13.7 [9]
8/7/2018 InP#1807 0.81 8.0 [10]
5/22/2018 InP#1806 0.88 8.4 [11]
4/26/2018 InP#1805 1.29 13.6 [12]
4/10/2018 InP#1804 1.12 12.8 [13]
4/5/2018 InP#1803 1.05 11.9 [14]
3/1/2018 InP#1802 0.96 9 [15]
1/2/2018 InP#1801 1.44 14.3 [16]
12/7/2017 InP#1714 0.96 10.4 [17]
11/21/2017 InP#1713 1.04 12.1 [18]
10/23/2017 InP#1712 1.11 13.1 [19]
10/11/2017 InP#1711 1 11 [20]
8/28/2017 InP#1710 1 11.7 [21]
8/16/2017 InP#1709 0.76 8 [22]
7/6/2017 InP#1708 0.98 12.1 [23]
5/19/2017 InP#1707 0.82 9.9 [24]
5/4/2017 InP#1706 0.84 11 [25]
4/20/2017 inP#1705 0.88 10.2 [26]
3/21/2017 InP#1704 1.01 11.3 [27]
2/21/2017 InP#1703 0.91 11.3 [28]
2/7/2017 InP#1702 0.75 7.7 [29]
1/23/2017 InP#1701 0.93 9.4 [30]
12/15/2016 InP#1615 0.91 9.3 [31]
12/1/2016 InP#1614 0.96 12.1 [32]
10/4/2016 InP#1613 0.92 8.9 [33]