ICP#2: 0.5Pa, 50/500W, CHF3/CF4/O2=35/5/10sccm, time=210 sec
Date Sample# Etch Rate (nm/min) Etch Selectivity (SiO2/PR) Averaged Sidewall Angle (o) SEM Images
10/5/2018 SiO2#01 95.2 0.74 77.9 [1]
1/28/2019 I21902 92.1 0.77 [2]
3/6/2019 I21903 88.5 0.80 79.4 [3]