ICP#1: 0.5Pa, 50/500W, CHF3/CF4/O2=35/5/10sccm, time=210 sec
Date Sample# Etch Rate (nm/min) Etch Selectivity (SiO2/PR) Averaged Sidewall Angle (o) SEM Images
1/28/2019 I11902 78.1 0.63 [1]
5/29/2019 I11904 71.1 0.58 [2]