{| class="wikitable"
| colspan="5" |ICP#1: 0.5Pa, 50/900W, CHF3/CF4=10/30 sccm, time=210 sec
+
|+'''ICP#1 Recipe:'''
|
+
0.5Pa, 50/900W, CHF3/CF4=10/30 sccm, time=210 sec
 
|-
 
|-
|Date
+
|'''Date'''
|Sample#
+
|'''Sample#'''
|Etch  Rate (nm/min)
+
|'''Etch  Rate (nm/min)'''
|Etch  Selectivity (SiO2/PR)
+
|'''Etch  Selectivity (SiO2/PR)'''
|Averaged  Sidewall Angle (<sup>o</sup>)
+
|'''Averaged  Sidewall Angle (<sup>o</sup>)'''
|SEM Images
+
|'''SEM Images'''
 
|-
 
|-
 
|1/28/2019
 
|1/28/2019
Line 14: Line 14:
 
|110
 
|110
 
|1.35
 
|1.35
|
+
|see SEM →
|[https://www.nanotech.ucsb.edu/wiki/images/b/b1/I11901.pdf]
+
|[https://wiki.nanotech.ucsb.edu/wiki/images/b/b1/I11901.pdf]
 
|-
 
|-
 
|5/29/2019
 
|5/29/2019
Line 22: Line 22:
 
|1.41
 
|1.41
 
|
 
|
|[https://www.nanotech.ucsb.edu/wiki/images/c/c6/I11903.pdf]
+
|[https://wiki.nanotech.ucsb.edu/wiki/images/c/c6/I11903.pdf]
 
|-
 
|-
 
|1/13/2020
 
|1/13/2020
Line 28: Line 28:
 
|78.0
 
|78.0
 
|1.06
 
|1.06
|
+
|unusual - two regions
 
|[https://wiki.nanotech.ucsb.edu/wiki/images/b/bb/I1200107.pdf]
 
|[https://wiki.nanotech.ucsb.edu/wiki/images/b/bb/I1200107.pdf]
 
|-
 
|-
| colspan="6" |Rate on 1/13/2020 is low by ~20%, so chamber was wet-cleaned on 1/21/2020.  Data below for 1/23 shows rate returned to "normal".
+
| colspan="6" |''Rate on 1/13/2020 is low by ~20%, so chamber was wet-cleaned on 1/21/2020.  Data below for 1/23 shows rate returned to "normal".''
 
|-
 
|-
 
|1/23/2020
 
|1/23/2020
Line 47: Line 47:
 
|[https://wiki.nanotech.ucsb.edu/wiki/images/e/ec/I1200301.pdf]
 
|[https://wiki.nanotech.ucsb.edu/wiki/images/e/ec/I1200301.pdf]
 
|-
 
|-
| colspan="6" |Sidewall profile on 2/28/2020 etches is slanted, chamber will be wet-cleaned on 3/24/2020 and re-tested.
+
| colspan="6" |''Sidewall profile on 2/28/2020 etches is slanted, chamber will be wet-cleaned on 3/2/2020 and re-tested. Data below shows etch returned to "normal".''
 
|-
 
|-
 
|3/3/2020
 
|3/3/2020
Line 54: Line 54:
 
|1.05
 
|1.05
 
|
 
|
 +
|[https://wiki.nanotech.ucsb.edu/w/images/b/b3/I1200415.pdf]
 +
|-
 +
|1/7/2021
 +
|I12101
 +
|118
 +
|1.12
 
|
 
|
 +
|[https://wiki.nanotech.ucsb.edu/w/images/4/49/I1210113.pdf]
 
|}
 
|}

Latest revision as of 19:39, 8 January 2021

ICP#1 Recipe: 0.5Pa, 50/900W, CHF3/CF4=10/30 sccm, time=210 sec
Date Sample# Etch Rate (nm/min) Etch Selectivity (SiO2/PR) Averaged Sidewall Angle (o) SEM Images
1/28/2019 I11901 110 1.35 see SEM → [1]
5/29/2019 I11903 105 1.41 [2]
1/13/2020 I12001 78.0 1.06 unusual - two regions [3]
Rate on 1/13/2020 is low by ~20%, so chamber was wet-cleaned on 1/21/2020. Data below for 1/23 shows rate returned to "normal".
1/23/2020 I12002 109 1.16 [4]
2/28/2020 I12003 119 1.17 56.6 [5]
Sidewall profile on 2/28/2020 etches is slanted, chamber will be wet-cleaned on 3/2/2020 and re-tested. Data below shows etch returned to "normal".
3/3/2020 I12004 110 1.05 [6]
1/7/2021 I12101 118 1.12 [7]