Difference between revisions of "Test Data of etching SiO2 with CHF3/CF4"

From UCSB Nanofab Wiki
Jump to navigation Jump to search
(add data)
Line 13: Line 13:
 
|1.2
 
|1.2
 
|82.1
 
|82.1
 +
|-
 +
|1/28/2019
 +
|I21901
 +
|146
 +
|1.2
 +
|
 
|}
 
|}
 
[https://www.nanotech.ucsb.edu/wiki/index.php/File:SiO2_Etch_using_ICP2-no_O2.pdf File:SiO2 Etch using ICP2-no O2.pdf]
 
[https://www.nanotech.ucsb.edu/wiki/index.php/File:SiO2_Etch_using_ICP2-no_O2.pdf File:SiO2 Etch using ICP2-no O2.pdf]

Revision as of 10:16, 29 January 2019

ICP#2: 0.5Pa, 50/900W, CHF3/CF4=10/30 sccm, time=210 sec
Date Sample# Etch Rate (nm/min) Etch Selectivity (SiO2/PR) Averaged Sidewall Angle (o)
10/5/2018 SiO2#02 160 1.2 82.1
1/28/2019 I21901 146 1.2

File:SiO2 Etch using ICP2-no O2.pdf