Difference between revisions of "Sputtering Recipes"
(Text replacement - "www.nanotech.ucsb.edu/wiki/" to "wiki.nanotech.ucsb.edu/wiki/") |
(→Sputter 4 (AJA ATC 2200-V): added Ru ; link to SiO2 Etching with Ruthenium Hardmask doc.) |
||
(2 intermediate revisions by the same user not shown) | |||
Line 229: | Line 229: | ||
|Pt||3 |
|Pt||3 |
||
| ||50(439V)||0||20||45||0||0||H2.75-T5||3.9||-||-||-||-||Yes||Ning Cao |
| ||50(439V)||0||20||45||0||0||H2.75-T5||3.9||-||-||-||-||Yes||Ning Cao |
||
+ | |- |
||
+ | |Ru |
||
+ | |3 |
||
+ | | |
||
+ | |200 |
||
+ | | |
||
+ | | |
||
+ | |45 |
||
+ | | |
||
+ | | |
||
+ | |H2.75-T4 |
||
+ | |~10 |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | | |
||
+ | |Yes |
||
+ | |Ning Cao |
||
|- |
|- |
||
|Ti||10 |
|Ti||10 |
||
Line 250: | Line 268: | ||
|} |
|} |
||
⚫ | |||
− | |||
⚫ | |||
− | |||
⚫ | |||
− | |||
⚫ | |||
− | |||
⚫ | |||
− | |||
⚫ | |||
− | |||
⚫ | |||
− | |||
⚫ | |||
− | |||
⚫ | |||
− | |||
⚫ | |||
==Au Deposition (Sputter 4)== |
==Au Deposition (Sputter 4)== |
||
Line 285: | Line 284: | ||
**B = 5.980E-3 |
**B = 5.980E-3 |
||
**C = 1.622E-4 |
**C = 1.622E-4 |
||
+ | |||
⚫ | |||
+ | |||
⚫ | |||
+ | |||
+ | == Ru Deposition (Sputter 4) == |
||
+ | * [https://wiki.nanotech.ucsb.edu/w/images/f/f6/SiO2_Etch%2C_Ru_HardMask_-_Fluorine_ICP_Etch_Process_-_Ning_Cao_2019-06.pdf Ruthenium Hardmask for SiO2 Etching - Full Process Traveler] by Ning Cao |
||
+ | ** Deposition Rate ~10nm/min |
||
+ | ** See [[ICP Etching Recipes#SiO2 Etching|Fluorine-ICP > SiO2 Etching]] page for more info. |
||
+ | |||
⚫ | |||
+ | |||
⚫ | |||
+ | |||
⚫ | |||
+ | |||
⚫ | |||
+ | |||
⚫ | |||
+ | |||
⚫ | |||
⚫ | |||
+ | |||
⚫ | |||
=[[Sputter 5 (AJA ATC 2200-V)]]= |
=[[Sputter 5 (AJA ATC 2200-V)]]= |
||
Line 465: | Line 488: | ||
− | [[Sputter 2 (SFI Endeavor)|<big> |
+ | = [[Sputter 2 (SFI Endeavor)|<big><u>Sputter 2 (SFI Endeavor)</u></big>]] = |
− | |||
'''This Tool has been Disabled, and is not available for use any more! These recipes are displayed here for historical/reference purposes only.''' |
'''This Tool has been Disabled, and is not available for use any more! These recipes are displayed here for historical/reference purposes only.''' |
||
Revision as of 10:47, 12 January 2021
Back to Vacuum Deposition Recipes. R
Sputter 3 (AJA ATC 2000-F)
The recipes below are given as starting points from data obtained in the nanofab. For critical depositions, calibrations are recommended. Please see the SignupMonkey Page for a list of currently installed targets.
Material | P(mT) | Pow(W) | Sub(W) | T(C) | Ar | N2 | O2 | Height-Tilt | Rate(nm/min) | Stress(MPa) | Rs(uOhm-cm) | n@633nm | k@633nm | Target Consumed Lower Limit | Data Below | Comment |
---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
Au | - | - | - | - | - | - | - | - | - | - | - | - | - | Set: 200 W
Read: 400 VDC |
no | |
Al2O3 | 3 | 200 (RF2) | off | 20 | 30 | 1.5 | 1.52"-4mm | 5.32 | 1.6478 | 0 | no | Demis D. John | ||||
Co | 10(5) | 200 | 0 | 20 | 25 | 0 | 0 | 25-9 | 2.3 | - | - | - | - | yes | Alex K | |
Cr | 5 | 200 | 0 | 20 | 25 | 0 | 0 | 44-4 | 6.84 | - | - | - | - | no | Brian | |
Cu | 1.5 | 50(395v) | 0 | 20 | 25 | 0 | 0 | 25-9 | 4.15 | - | - | - | - | no | Ning | |
Cu | 5 | 150(~490v) | 0 | 20 | 15 | 0 | 0 | 0.82"-9 | 8 | - | - | - | - | yes | Ning | |
Fe | 10(5) | 200 | 0 | 20 | 25 | 0 | 0 | 25-9 | 1.25 | - | - | - | - | No | Alex K | |
Mo | 3 | 200 | 0 | 20 | 25 | 0 | 0 | 44-4 | 13.15 | - | - | - | - | yes | Ning | |
Ni | 5 | 150 | 0 | 20 | 25 | 0 | 0 | 44-4 | 5.23 | - | - | - | - | yes | Ning | |
Ni | 5 | 150 | 0 | 20 | 25 | 0 | 0 | 25-9 | 1.82 | - | - | - | - | yes | Ning | |
Ni | 5 | 75 | 0 | 20 | 25 | 0 | 0 | 44-4 | 2.50 | - | - | - | - | yes | Ning | |
Ni | 3 | 200 | 0 | 20 | 25 | 0 | 0 | 44-4 | 9.4 | - | - | - | - | yes | Ning | |
Ni | 1.5 | 50(399v) | 0 | 20 | 25 | 0 | 0 | 25-9 | 0.96 | - | - | - | - | no | Ning | |
Pt | 3 | 50 | 0 | 20 | 25 | 0 | 0 | 0.82"-9 | 2.9 | - | - | - | - | no | Ning | |
Si | 8 | 250 | 0 | 25 | 25 | 0 | 0 | 15-3 | 1.4 | - | - | - | - | no | Gerhard - ramp 2W/s - 3% Unif 4" wafer | |
SiN | 3 | 200 | 10 | 20 | 25 | 3 | 0 | 25-9 | 1.56 | - | - | 1.992 | - | yes | Brian | |
SiN | 3 | 250 | 10 | 20 | 25 | 2.5 | 0 | 25-9 | 2.1 | - | - | 2.06 | - | yes | Brian | |
SiO2 | 3 | 200 | 10 | 20 | 25 | 0 | 3 | 25-9 | 3.68 | - | - | 1.447 | - | yes | Brian | |
SiO2 | 3 | 200 | 10 | 20 | 25 | 0 | 5 | 45-3 | 2.60 | - | - | 1.471 | - | yes | Brian | |
SiO2 | 3 | 250 | 10 | 20 | 25 | 0 | 2.5 | 25-9 | 4.3 | - | - | 1.485 | - | yes | Brian | |
Ta | 5 | 150 | 0 | 20 | 25 | 0 | 0 | 44-4 | 9.47 | - | - | - | - | yes | Ning | |
Ta | 5 | 75 | 0 | 20 | 25 | 0 | 0 | 44-4 | 5.03 | - | - | - | - | yes | Ning | |
Ti | 3 | 100 | 0 | 20 | 25 | 0 | 0 | 25-9 | 1.34 | - | - | - | - | yes | Ning | |
SampleClean-NativeSiO2 | 10 | 0 | 18 | 20 | 25 | 0 | 0 | 44-4 | - | - | - | - | - | yes | 150Volts 5 min |
Height Conversion for Older Recipes
Old recipes using the manual Height setting in millimeters can be converted to the new programmatic settings in inches as follows:
Old (mm) | New (inches) | Typical Gun Tilt (mm) |
---|---|---|
15 | ||
25 | 0.82 | 9 |
44 | 1.52 | 4 |
Interpolation plot can be found here.
Fe and Co Deposition (Sputter 3)
Cu Deposition (Sputter 3)
Mo Deposition (Sputter 3)
Ni and Ta Deposition (Sputter 3)
SiO2 Deposition (Sputter 3)
SiN Deposition (Sputter 3)
Ti Deposition (Sputter 3)
Sputter 4 (AJA ATC 2200-V)
The recipes below are given as starting points from data obtained in the nanofab. For critical depositions, calibrations are recommended. Please see the SignupMonkey page for a list of currently installed targets.
Material | P(mT) | Power Source | Pow(W) | Sub(W) | T(C) | Ar | N2 | O2 | Height-Tilt | Rate(nm/min) | Stress(MPa) | Rs(uOhm-cm) | n@633nm | k@633nm | Data Below | Comment |
---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
Al | 5 | 200 | 0 | 20 | 45 | 0 | 0 | H2.75-T5 | 4.4 | - | - | - | - | Yes | Ning Cao | |
Al2O3 | 3 | RF4-Sw1 | 200 | 0 | 20 | 30 | 0 | 1.5 | H2.75-T5 | 5.1 | 1.64202 | 0 | partial | Demis D. John | ||
Au | 5 | 200 | 0 | 20 | 45 | 0 | 0 | H1-T10 | 17.7 | - | - | - | - | Yes | Ning Cao | |
Au | 10 | 300 | 0 | 20 | 45 | 0 | 0 | H2.75-T5 | 45.4 | - | - | - | - | Yes | Ning Cao | |
Cu | 5 | 150 | 0 | 20 | 30 | 0 | 0 | H0.82-T9 | 6.7 | No (SEM available) | Ning Cao | |||||
Nb | 4 | 250 | 0 | 20 | 30 | 0 | 0 | H2.00-T7 | 7.5 | - | - | - | - | No | ||
Pt | 5 | 200 | 0 | 20 | 45 | 0 | 0 | H2.75-T5 | 7.4 | - | - | - | - | Yes | Ning Cao | |
Pt | 3 | 50(439V) | 0 | 20 | 45 | 0 | 0 | H2.75-T5 | 3.9 | - | - | - | - | Yes | Ning Cao | |
Ru | 3 | 200 | 45 | H2.75-T4 | ~10 | Yes | Ning Cao | |||||||||
Ti | 10 | 200 | 0 | 20 | 45 | 0 | 0 | H2.75-T5 | 2.3 | - | - | - | - | Yes | Ning Cao | |
TiN | 3 | 150 | 110V | 20 | 48.25 | 1.75 | 0 | H2.5-T5 | 2 | - | 60 | - | - | No | ||
TiO2 | 3 | 250(RF:450V) | 0 | 20 | 45 | 0 | 3 | H2.75-T5 | 4.3 | - | - | - | Yes | Ning Cao | ||
TiW | 4.5 | 200 | 0 | 20 | 45 | 0 | 0 | H1-T10 | 4.7 | - | - | - | - | Yes | Ning Cao | |
TiW | 4.5 | 300 | 0 | 75 | 45 | 0 | 0 | H2.75-T5 | 9.5 | -150 to 150 | 60 | - | - | Yes | 10%Ti by Wt | |
W | 3 | 300 | 0 | 50 | 45 | 0 | 0 | H2.75-T5 | 11.5 | -150 to 150 | 11 | - | - | Yes | Jeremy Watcher |
Au Deposition (Sputter 4)
Al Deposition (Sputter 4)
Al2O3 Deposition (Sputter 4)
- Rate: 5.134 nm/min
- Cauchy Refractive Index Params (fit from λ=190-1700nm, indicating transparency over this range)
- A = 1.626
- B = 5.980E-3
- C = 1.622E-4
Pt Deposition (Sputter 4)
Ru Deposition (Sputter 4)
- Ruthenium Hardmask for SiO2 Etching - Full Process Traveler by Ning Cao
- Deposition Rate ~10nm/min
- See Fluorine-ICP > SiO2 Etching page for more info.
Ti-Au Deposition (Sputter 4)
TiO2 Deposition (Sputter 4)
TiW Deposition (Sputter 4)
W-TiW Deposition (Sputter 4)
Sputter 5 (AJA ATC 2200-V)
The recipes below are given as starting points from data obtained in the nanofab. For critical depositions, calibrations are recommended.
Please see the SignupMonkey page for a list of currently installed targets.
Material | P(mT) | Power Source | Pow(W) | Sub(V) | T(C) | Ar | N2 | O2 | Height-Tilt | Rate(nm/min) | Stress(MPa) | Rs(uOhm-cm) | Rq(nm) | n@633nm | k@633nm | LPDb/LPDa* | Data Below | Comment |
---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
Al | 5 | 250 | 0 | 20 | 45 | 0 | 0 | H1-T10 | 2.5 | 22 | No (SEM available) | Ning | ||||||
Al2O3 | 1.5 | DC5-SW1 | 150 | - | - | 45 | - | 5 | H2.75-T5 | 5.3 | ? | ? | ? | 1.641 | - | ? | No | Demis 2018-04-13 |
SiO2 | 3 | 250 | 120 | 20 | 45 | 0 | 2 | H1.0-T10 | 2.32 | - | - | 1.49 | - | 153/6384 | No | Biljana | ||
SiO2 | 3 | 250 | 120 | 20 | 45 | 0 | 4.5 | H1.0-T10 | 2.29 | -515 | - | 0.210 | 1.49 | 138/4445 | No ( AFM available) | Biljana | ||
SiO2 | 3 | 250 | 120 | 20 | 45 | 0 | 6 | H1.0-T10 | 2.32 | - | - | 1.49 | - | 27/1515 | Yes | Biljana |
*LPD: light particle detection:
- LPDb: light particle detection before deposition
- LPDa: light particle detection after deposition
SiO2 Deposition (Sputter 5)
Ion Beam Deposition (Veeco NEXUS)
- IBD Calibrations Spreadsheet - Records of historical film depositions (rates, indices), Uniformity etc.
- All users are required to enter their calibration deps (simple test deps only)
- Particulates in SiO2 and Ta2O5 in 2015
SiO2 deposition (IBD)
- SiO2 Standard Recipe
- SiO2 Data December 2014
- SiO2 Thickness uniformity 2014
- SiO2 Data-15min depositions 2015
- SiO2 Thickness uniformity-15 min depositions 2015
- SiO2 Data-1hr depositions 2015
- SiO2 Thickness uniformity-1hr depositions 2015
- SiO2 Data-1hr depositions 2016
- SiO2 Thickness uniformity-1hr depositions 2016
SiO2 1hr deposition properties:
- Dep.rate: ≈ 5.2 nm/min (users must calibrate this prior to critical deps)
- HF e.r.~350 nm/min
- Stress ≈ -390MPa (compressive)
- Refractive Index: ≈ 1.494
- [Cauchy Parameters] (350-2000nm):
- A = 1.480
- B = 0.00498
- C = -3.2606e-5
Si3N4 deposition (IBD)
- Deposition Rate: ≈ 4.10 nm/min (users must calibrate this prior to critical deps)
- HF e.r.~11nm/min
- Stress ≈ -1590MPa (compressive)
- Refractive Index: ≈ 1.969
- [Cauchy Parameters] (350-2000nm):
- A = 2.000
- B = 0.01974
- C = 1.2478e-4
SiOxNy deposition (IBD)
These are some old (2010), initial characterizations only. A recipe improvement would be to increase the Assist O2+N2 = 60sccm total, increasing repeatability. Contact Demis for more info.
Ta2O5 deposition (IBD)
- Ta2O5 Data December-15 min depositions 2015
- Ta2O5 Thickness uniformity-15 min depositions 2015
- Ta2O5 Data December-1hr depositions 2015
- Ta2O5 Thickness uniformity-1hr depositions 2015
- Ta2O5 Data December-1hr depositions 2016
- Ta2O5 Thickness uniformity-1hr depositions 2016
- Ta2O5 1hr depositions:
- Deposition Rate: ≈ 7.8 nm/min (users must calibrate this prior to critical deps)
- HF e.r.~2 nm/min
- Stress ≈ -232MPa (compressive)
- Refractive Index: ≈ 2.172
- [Cauchy Parameters] (350-2000nm):
- A = 2.1123
- B = 0.018901
- C = -0.016222
TiO2 deposition (IBD)
- Deposition Rate: ≈ 1.29 nm/min (users must calibrate this prior to critical deps)
- HF etch rate ~5.34nm/min
- Stress ≈ -445MPa (compressive)
- Refractive Index: ≈ 2.259
- [Cauchy Parameters] (350-2000nm):
- A = 2.435
- B = -4.9045e-4
- C = 0.01309
- Absorbing < ~350nm
Al2O3 deposition (IBD)
- Al2O3 standard recipe: 1_Al2O3_dep
- Deposition Rate: ≈ 2.05nm/min (users must calibrate this prior to critical deps)
- HF etch rate ~167nm/min
- Stress ≈ -332MPa (compressive)
- Refractive Index: ≈ 1.656
- [Cauchy Parameters] (350-2000nm):( working on)
- A =
- B =
- C =
- Absorbing < ~350nm
Sputter 2 (SFI Endeavor)
This Tool has been Disabled, and is not available for use any more! These recipes are displayed here for historical/reference purposes only.