=[[PECVD 1 (PlasmaTherm 790)]]=
 
=[[PECVD 1 (PlasmaTherm 790)]]=
  
===[https://docs.google.com/spreadsheets/d/1fTDNXxpf4tgNYLIEs_jvehG1KvtXqqTRDBI7sHNAVvo/edit#gid=1270764394 PECVD 1 Plots] - SiO2, SiN and Particulate Count===
+
===[https://docs.google.com/spreadsheets/d/1fTDNXxpf4tgNYLIEs_jvehG1KvtXqqTRDBI7sHNAVvo/edit#gid=1270764394 PECVD 1 Process Control Plots] - Plots of all process control data===
  
 
==SiO<sub>2</sub> deposition (PECVD #1)==
 
==SiO<sub>2</sub> deposition (PECVD #1)==
  
*[https://docs.google.com/spreadsheets/d/1uqpg3sirsRbXdTFlxZ6_k3t0ovP0MtpFtICjpH0-prs/edit#gid= SiO<sub>2</sub><nowiki> [PECVD 1] Standard Recipe</nowiki>]
+
 
 +
*[https://docs.google.com/spreadsheets/d/1wloq6HJw5RQIvmeKcBn3xvE_917R6jF_K-btCHjsiIM/edit#gid= SiO<sub>2</sub><nowiki> [PECVD 1] Standard Recipe</nowiki>]
 +
 
 
*[https://docs.google.com/spreadsheets/d/1fTDNXxpf4tgNYLIEs_jvehG1KvtXqqTRDBI7sHNAVvo/edit#gid=0 SiO<sub>2</sub><nowiki> [PECVD 1] Current Process Control Data</nowiki>]
 
*[https://docs.google.com/spreadsheets/d/1fTDNXxpf4tgNYLIEs_jvehG1KvtXqqTRDBI7sHNAVvo/edit#gid=0 SiO<sub>2</sub><nowiki> [PECVD 1] Current Process Control Data</nowiki>]
 
*[https://docs.google.com/spreadsheets/d/1fTDNXxpf4tgNYLIEs_jvehG1KvtXqqTRDBI7sHNAVvo/edit#gid=1503619544 SiO<sub>2</sub><nowiki> [PECVD 1] Historical Data</nowiki>] - Oct. 2021 and earlier
 
*[https://docs.google.com/spreadsheets/d/1fTDNXxpf4tgNYLIEs_jvehG1KvtXqqTRDBI7sHNAVvo/edit#gid=1503619544 SiO<sub>2</sub><nowiki> [PECVD 1] Historical Data</nowiki>] - Oct. 2021 and earlier
Line 20: Line 22:
  
 
*[https://wiki.nanotech.ucsb.edu/wiki/images/4/4a/New_PECVD1-LS_SIN-Turner05recipe_2014_LS_SIN_recipe.pdf Low Stress Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 1] Standard Recipe</nowiki>]
 
*[https://wiki.nanotech.ucsb.edu/wiki/images/4/4a/New_PECVD1-LS_SIN-Turner05recipe_2014_LS_SIN_recipe.pdf Low Stress Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 1] Standard Recipe</nowiki>]
*[https://docs.google.com/spreadsheets/d/1fTDNXxpf4tgNYLIEs_jvehG1KvtXqqTRDBI7sHNAVvo/edit#gid=1515630363 Low Stress Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 1] Current Process Control Data</nowiki>]
+
*[[To Be Added|Low Stress Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 1] Current Process Control Data</nowiki>]] ''- To Be Added''
 
*[https://docs.google.com/spreadsheets/d/1fTDNXxpf4tgNYLIEs_jvehG1KvtXqqTRDBI7sHNAVvo/edit#gid=934830479 Low Stress Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 1] Historical Data</nowiki>] - 2021-10 and earlier
 
*[https://docs.google.com/spreadsheets/d/1fTDNXxpf4tgNYLIEs_jvehG1KvtXqqTRDBI7sHNAVvo/edit#gid=934830479 Low Stress Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 1] Historical Data</nowiki>] - 2021-10 and earlier
  
Line 26: Line 28:
  
 
*[https://wiki.nanotech.ucsb.edu/wiki/images/2/24/New_PECVD1-LS_SION-recipe_2014_LS_SION_recipe.pdf SiO<sub>x</sub>N<sub>y</sub> Standard Recipe]
 
*[https://wiki.nanotech.ucsb.edu/wiki/images/2/24/New_PECVD1-LS_SION-recipe_2014_LS_SION_recipe.pdf SiO<sub>x</sub>N<sub>y</sub> Standard Recipe]
*[https://docs.google.com/spreadsheets/d/1rixyzAAq6q08M5OwvZiDVoh3K8B566XKM-UZAQIAnsg/edit#gid=sharing SiO<sub>x</sub>N<sub>y</sub> Data 2014]
+
*[https://docs.google.com/spreadsheets/d/1rixyzAAq6q08M5OwvZiDVoh3K8B566XKM-UZAQIAnsg/edit#gid=sharing SiO<sub>x</sub>N<sub>y</sub> Data 2014] - ''Rate, Index etc.''
 
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dEttR2JSTkRoamR0SUZ4bE5QUW9uS2c&usp=sharing SiO<sub>x</sub>N<sub>y</sub>1000A Thickness uniformity 2014]
 
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dEttR2JSTkRoamR0SUZ4bE5QUW9uS2c&usp=sharing SiO<sub>x</sub>N<sub>y</sub>1000A Thickness uniformity 2014]
  
Line 58: Line 60:
 
=[[PECVD 2 (Advanced Vacuum)]]=
 
=[[PECVD 2 (Advanced Vacuum)]]=
  
===[https://docs.google.com/spreadsheets/d/1iSW1eAAg824y9PYYLG9aiaw53PEJ-f9ofylpVlCDq9Y/edit#gid=272916741 PECVD 2 Plots]===
+
===[https://docs.google.com/spreadsheets/d/1iSW1eAAg824y9PYYLG9aiaw53PEJ-f9ofylpVlCDq9Y/edit#gid=272916741 PECVD 2 Process Control Plots] - Plots of all process control data===
  
 
==SiO<sub>2</sub> deposition (PECVD #2)==
 
==SiO<sub>2</sub> deposition (PECVD #2)==
Line 73: Line 75:
  
 
==Low-Stress SiN deposition (PECVD #2)==
 
==Low-Stress SiN deposition (PECVD #2)==
''Low-Stress SilIcon Nitride, Si<sub>3</sub>N<sub>4</sub> (< 100 MPa)''
+
''Low-Stress Silicon Nitride, Si<sub>3</sub>N<sub>4</sub> (< ±100 MPa)''
 +
 
 +
*[https://docs.google.com/spreadsheets/d/1DzzI7aE61R7c6gyk6cGBdm9FtGrApiNJ4AL90ll2C8k/edit#gid= Low Stress Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 2] Standard Recipe</nowiki>] - "''LSNitride2''
  
*[https://docs.google.com/spreadsheets/d/1DzzI7aE61R7c6gyk6cGBdm9FtGrApiNJ4AL90ll2C8k/edit#gid= Low Stress Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 2] Standard Recipe</nowiki>] - "''LSNitride2''"
 
***''Old Versions of the recipe:''
 
****[https://wiki.nanotech.ucsb.edu/wiki/images/a/a5/New_AdvPECVD-LS_Nitride2_300C_standard_recipe_LS_Nitride2_standard_recipe.pdf LS Nitride2 Standard Recipe 2014-5/9/2018]
 
****[https://wiki.nanotech.ucsb.edu/wiki/images/0/01/STD_LSNitride2_5-9-18.pdf STD LSNitride2 5/9/2018]
 
 
*[https://docs.google.com/spreadsheets/d/1iSW1eAAg824y9PYYLG9aiaw53PEJ-f9ofylpVlCDq9Y/edit#gid=584923738 Low Stress Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 2] Current Process Control Data</nowiki>]
 
*[https://docs.google.com/spreadsheets/d/1iSW1eAAg824y9PYYLG9aiaw53PEJ-f9ofylpVlCDq9Y/edit#gid=584923738 Low Stress Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 2] Current Process Control Data</nowiki>]
*[https://docs.google.com/spreadsheets/d/1iSW1eAAg824y9PYYLG9aiaw53PEJ-f9ofylpVlCDq9Y/edit#gid=268003895 Low Stress Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 2] Historical Data - Before Oct. 2021</nowiki>]
+
*[https://docs.google.com/spreadsheets/d/1iSW1eAAg824y9PYYLG9aiaw53PEJ-f9ofylpVlCDq9Y/edit#gid=203400760 Plots of Low-Stress Si<sub>3</sub>N<sub>4</sub> Process Control Data]
 +
*[[To Be Added|Low Stress Si<sub>3</sub>N<sub>4</sub><nowiki> [PECVD 2] Historical Data - Before Oct. 2021</nowiki>]]
 +
*:''Old Versions of the recipe:''
 +
*:''[https://wiki.nanotech.ucsb.edu/wiki/images/a/a5/New_AdvPECVD-LS_Nitride2_300C_standard_recipe_LS_Nitride2_standard_recipe.pdf LS Nitride2 Standard Recipe 2014-5/9/2018]''
 +
*:''[https://wiki.nanotech.ucsb.edu/wiki/images/0/01/STD_LSNitride2_5-9-18.pdf STD LSNitride2 5/9/2018]''
  
 
==Amorphous-Si deposition (PECVD #2)==
 
==Amorphous-Si deposition (PECVD #2)==
Line 119: Line 123:
 
  The system currently has '''Deuterated Silane (SiD<sub>4</sub>)''' installed - identical to the regular Silicon precursor SiH<sub>4</sub>, except that it significantly lowers optical absorption in the near-infrared due to shifted molecular vibrations/molecular weights. This gas is more expensive and thus more applicable to optical application than to general-purpose SiN films.
 
  The system currently has '''Deuterated Silane (SiD<sub>4</sub>)''' installed - identical to the regular Silicon precursor SiH<sub>4</sub>, except that it significantly lowers optical absorption in the near-infrared due to shifted molecular vibrations/molecular weights. This gas is more expensive and thus more applicable to optical application than to general-purpose SiN films.
  
===[https://docs.google.com/spreadsheets/d/1CuDMKFTTzGLL6CP-FEI_9cOnUaIw-432ppDFssB59wY/edit#gid=417334948https://docs.google.com/spreadsheets/d/1CuDMKFTTzGLL6CP-FEI_9cOnUaIw-432ppDFssB59wY/edit#gid=417334948 ICP-PECVD Plots] - TBD===
+
===[https://docs.google.com/spreadsheets/d/1CuDMKFTTzGLL6CP-FEI_9cOnUaIw-432ppDFssB59wY/edit#gid=417334948https://docs.google.com/spreadsheets/d/1CuDMKFTTzGLL6CP-FEI_9cOnUaIw-432ppDFssB59wY/edit#gid=417334948 ICP-PECVD Process Control Plots] - Plots of all Process Control data===
  
 
==Low Deposition Rate SiO<sub>2</sub> [ICP-PECVD]==
 
==Low Deposition Rate SiO<sub>2</sub> [ICP-PECVD]==
Line 136: Line 140:
  
 
*[https://docs.google.com/spreadsheets/d/1VrgS0cB2OcdZVTCnDAesgQCLRaAgEB_Iajc_OrhXOo0/edit#gid=1199123007 Si<sub>3</sub>N<sub>4</sub><nowiki> [ICP-PECVD] Standard Recipe</nowiki>] - "''SiN 250C''"
 
*[https://docs.google.com/spreadsheets/d/1VrgS0cB2OcdZVTCnDAesgQCLRaAgEB_Iajc_OrhXOo0/edit#gid=1199123007 Si<sub>3</sub>N<sub>4</sub><nowiki> [ICP-PECVD] Standard Recipe</nowiki>] - "''SiN 250C''"
*[https://docs.google.com/spreadsheets/d/1CuDMKFTTzGLL6CP-FEI_9cOnUaIw-432ppDFssB59wY/edit#gid=1459210138 Si<sub>3</sub>N<sub>4</sub><nowiki> [ICP-PECVD] Current Process Control Data</nowiki>]
+
*[https://docs.google.com/spreadsheets/d/1CuDMKFTTzGLL6CP-FEI_9cOnUaIw-432ppDFssB59wY/edit#gid=1670372499 Si<sub>3</sub>N<sub>4</sub><nowiki> [ICP-PECVD] Current Process Control Data</nowiki>]
 
*[https://docs.google.com/spreadsheets/d/1CuDMKFTTzGLL6CP-FEI_9cOnUaIw-432ppDFssB59wY/edit#gid=782128304 Si<sub>3</sub>N<sub>4</sub><nowiki> [ICP-PECVD] Historical Data</nowiki>] - before Oct. 2021
 
*[https://docs.google.com/spreadsheets/d/1CuDMKFTTzGLL6CP-FEI_9cOnUaIw-432ppDFssB59wY/edit#gid=782128304 Si<sub>3</sub>N<sub>4</sub><nowiki> [ICP-PECVD] Historical Data</nowiki>] - before Oct. 2021
  
Line 142: Line 146:
  
 
*[https://docs.google.com/spreadsheets/d/1i2mE2K12EEulnCbO9KuU9PCcvHAmcGxTIXUF8x4IOWk/edit#gid=1199123007 Low Stress Si<sub>3</sub>N<sub>4</sub><nowiki> [ICP-PECVD] Standard Recipe</nowiki>] - "''SiN Low Stress 250C''"
 
*[https://docs.google.com/spreadsheets/d/1i2mE2K12EEulnCbO9KuU9PCcvHAmcGxTIXUF8x4IOWk/edit#gid=1199123007 Low Stress Si<sub>3</sub>N<sub>4</sub><nowiki> [ICP-PECVD] Standard Recipe</nowiki>] - "''SiN Low Stress 250C''"
*[https://docs.google.com/spreadsheets/d/1CuDMKFTTzGLL6CP-FEI_9cOnUaIw-432ppDFssB59wY/edit#gid=1459210138 Low Stress Si<sub>3</sub>N<sub>4</sub><nowiki> [ICP-PECVD] Current Process Control Data</nowiki>]
+
*[https://docs.google.com/spreadsheets/d/1CuDMKFTTzGLL6CP-FEI_9cOnUaIw-432ppDFssB59wY/edit#gid=1517031044 Low Stress Si<sub>3</sub>N<sub>4</sub><nowiki> [ICP-PECVD] Current Process Control Data</nowiki>]
 
*[https://docs.google.com/spreadsheets/d/1CuDMKFTTzGLL6CP-FEI_9cOnUaIw-432ppDFssB59wY/edit#gid=1024532473 Low Stress Si<sub>3</sub>N<sub>4</sub><nowiki> [ICP-PECVD] Historical Data</nowiki>] - before Oct. 2021
 
*[https://docs.google.com/spreadsheets/d/1CuDMKFTTzGLL6CP-FEI_9cOnUaIw-432ppDFssB59wY/edit#gid=1024532473 Low Stress Si<sub>3</sub>N<sub>4</sub><nowiki> [ICP-PECVD] Historical Data</nowiki>] - before Oct. 2021
  

Revision as of 16:30, 13 June 2022

Back to Vacuum Deposition Recipes.

PECVD 1 (PlasmaTherm 790)

PECVD 1 Process Control Plots - Plots of all process control data

SiO2 deposition (PECVD #1)

SiN deposition (PECVD #1)

Low Stress Si3N4 (PECVD#1)

SiOxNy deposition (PECVD #1)

Standard Cleaning Procedure (PECVD #1)

The cleaning procedure is very important in order to have consistent result on this tool and also to keep particulate count low. After each deposition you should clean the tool following instructions carefully. The clean is done in two steps:

  1. Wet cleaning (start cleaning by using a cleanroom wipe sprayed with DI. Wipe chamber sidewalls with it. Finish cleaning by using the cleanroom wipe sprayed with IPA. )
  2. Load the recipe for cleaning "CF4/O2 Clean" (edit the recipe and change ONLY time of cleaning). Follow instructions regarding a required time for cleaning.
Table of Cleaning Times
Film Dep'd Cleaning Time
SiO2 TBD
Si3N4 TBD
SiOxNy Same as XYZ

Standard Cleaning Recipe (PECVD#1): "CF4/O2 Clean"

Click the above link for a screenshot of the standard cleaning recipe, for which you will enter a custom time. The recipe is set up so that it will pop up a window for the cleaning time upon running the recipe - you do not need to edit the recipe before running it.

PECVD 2 (Advanced Vacuum)

PECVD 2 Process Control Plots - Plots of all process control data

SiO2 deposition (PECVD #2)

SiN deposition (PECVD #2)

Low-Stress SiN deposition (PECVD #2)

Low-Stress Silicon Nitride, Si3N4 (< ±100 MPa)

Amorphous-Si deposition (PECVD #2)

Standard Cleaning Procedure (PECVD #2)

The cleaning procedure is very important in order to have consistent result on this tool and also to keep particulate count low. After each deposition you should clean the tool following instructions carefully. The clean is done in two steps:

  1. (If >29min dep time) Wet cleaning: Start cleaning by using a cleanroom wipe sprayed with DI. Wipe upper chamber sidewalls with it. Finish cleaning by using the cleanroom wipe sprayed with IPA & wiping again.
  2. Load the recipe for cleaning "STD CF4/O2 Clean" (edit the recipe and change ONLY time of cleaning). Follow instructions regarding required time for cleaning.

Standard Clean Recipe (PECVD#2): "STD CF4/O2 Clean"

Click the above link for a screenshot of the standard cleaning recipe, for which you will enter a custom time. The recipe is set up so that it will pop up a window for the cleaning time upon running the recipe - you do not need to edit the recipe before running it.


Clean Times (PECVD#2)

Film Deposited Cleaning Time (Dry)
SiO2 1 min. clean for every 1 min. deposition
Si3N4 1 min. clean for every 7 min of deposition
If > 29min total dep time

(Season + Dep)

Wet Clean the Upper Lid/Chamber

DI water then Isopropyl Alcohol on chamber wall & portholes

ICP-PECVD (Unaxis VLR)

2020-02: New recipes have been characterized for low particulate count and repeatability.  Only staff-supplied recipes are allowed in the tool. Please follow the new procedures to ensure low particle counts in the chamber.
The system currently has Deuterated Silane (SiD4) installed - identical to the regular Silicon precursor SiH4, except that it significantly lowers optical absorption in the near-infrared due to shifted molecular vibrations/molecular weights. This gas is more expensive and thus more applicable to optical application than to general-purpose SiN films.

ICP-PECVD Process Control Plots - Plots of all Process Control data

Low Deposition Rate SiO2 [ICP-PECVD]

High Deposition Rate SiO2 [ICP-PECVD]

Si3N4 [ICP-PECVD]

Low Stress Si3N4 [ICP-PECVD]

Standard Cleaning Procedure [ICP-PECVD]

You must edit the Post-Dep Clean recipe to correspond to your deposited thickness and material. See the Operating Procedure on the Unaxis Tool Page for details.

  • SiNx etches at 20nm/min
  • SiO2 etches at 40nm/min

Standard Clean Recipe

To Be Added