Difference between revisions of "PECVD Recipes"

From UCSB Nanofab Wiki
Jump to navigation Jump to search
 
(54 intermediate revisions by 2 users not shown)
Line 10: Line 10:
 
*[https://docs.google.com/spreadsheets/d/1ct-SSCRxf81W0jupCWzh81n0DBwPv6mwKFMzuWu_0TI/edit#gid=sharing Particulates in PECVD#1 films 2019]
 
*[https://docs.google.com/spreadsheets/d/1ct-SSCRxf81W0jupCWzh81n0DBwPv6mwKFMzuWu_0TI/edit#gid=sharing Particulates in PECVD#1 films 2019]
 
*[https://docs.google.com/spreadsheets/d/1yks0OgH8rpbYjin_Qr8vpPg8jBiZQRs_PKfyfo-Rqg0/edit#gid=sharing Particulates in PECVD#1 films 2020]
 
*[https://docs.google.com/spreadsheets/d/1yks0OgH8rpbYjin_Qr8vpPg8jBiZQRs_PKfyfo-Rqg0/edit#gid=sharing Particulates in PECVD#1 films 2020]
 +
*[https://docs.google.com/spreadsheets/d/1vSmymaS_NNXW-ouC8Ky1J6iVSla7uyRB2zf1lGMa31g/edit#gid=sharing Particulates in PECVD#1 films 2021]
  
 
==SiN deposition (PECVD #1)==
 
==SiN deposition (PECVD #1)==
  
*[//wiki.nanotech.ucsb.edu/wiki/images/3/32/New_PECVD1-SiO2-standard_recipe_2014_SiO2_standard_recipe.pdf SiN Standard Recipe ( update this page)]
+
*[https://docs.google.com/spreadsheets/d/1DGU745SeunYz4sLs1LpGKbtOYX-tQyBHEvVYcMxHRKE/edit#gid= Si3N4 Standard Recipe]
*[https://docs.google.com/spreadsheets/d/10ccfgCf5O0JM6L9J5XDz-gWVQz9P24VU/edit#gid= Si3N4 Recipe parameters]
 
 
==== Historical Data ====
 
==== Historical Data ====
  
Line 26: Line 26:
 
*[https://docs.google.com/spreadsheets/d/1pAoTCaNSf0uZMyiQ2qKFd0s_e4e53P9Z1jUwtmTnlLk/edit#gid=sharing SiN 300nm Data 2018]
 
*[https://docs.google.com/spreadsheets/d/1pAoTCaNSf0uZMyiQ2qKFd0s_e4e53P9Z1jUwtmTnlLk/edit#gid=sharing SiN 300nm Data 2018]
 
*[https://docs.google.com/spreadsheets/d/1Pnw8eEaQ0rGblRYl6LeIm6wrh1hgeyjnHEbA4BzV8JM/edit#gid=sharing SiN 300nm Data 2019]
 
*[https://docs.google.com/spreadsheets/d/1Pnw8eEaQ0rGblRYl6LeIm6wrh1hgeyjnHEbA4BzV8JM/edit#gid=sharing SiN 300nm Data 2019]
*[https://docs.google.com/spreadsheets/d/1sx1_jvZnoQKY__8pl3nxjIcLrBHaCMQRyKyymDneLwc/edit#gid=sharing SiN 300nm Data 2020]
+
*[https://docs.google.com/spreadsheets/d/1N_1Kk6J-wA4nlHpFg5EMDZNHR1kLDo_fr_Dvc6osSr4/edit#gid=sharing SiN 300nm Data 2020]
 +
*[https://docs.google.com/spreadsheets/d/13jY5T_PW1a3GjHIbR0GuUbIhmxClQfvLgzaUtl3YniE/edit#gid=sharing SiN 300nm Data 2021]
  
 
===== Uniformity Data =====
 
===== Uniformity Data =====
Line 37: Line 38:
 
*[https://docs.google.com/spreadsheets/d/1b4EQZdRtVbqNwGBrItoG5-tz6RIzlsvBiCFR6ZXfylw/edit#gid=sharing SiN 300nm Thickness uniformity 2018]
 
*[https://docs.google.com/spreadsheets/d/1b4EQZdRtVbqNwGBrItoG5-tz6RIzlsvBiCFR6ZXfylw/edit#gid=sharing SiN 300nm Thickness uniformity 2018]
 
*[https://docs.google.com/spreadsheets/d/1-OiaH8frAzJzHKfbYTJP808ddzk1Wsv_CixDzG-sSfo/edit#gid=sharing SiN 300nm Thickness uniformity 2019]
 
*[https://docs.google.com/spreadsheets/d/1-OiaH8frAzJzHKfbYTJP808ddzk1Wsv_CixDzG-sSfo/edit#gid=sharing SiN 300nm Thickness uniformity 2019]
*[https://docs.google.com/spreadsheets/d/1eP6U2WJetu2wDB6wemkMPFG0JYx33I3Z3liihwae8Oo/edit#gid=sharing SiN 300nm Thickness uniformity 2020]
+
*[https://docs.google.com/spreadsheets/d/1e5ycwODa-VooEzGjhY4XquvJpuAuIQHHHZSRwZaH5-E/edit#gid=sharing SiN 300nm Thickness uniformity 2020]
 +
*[https://docs.google.com/spreadsheets/d/1Re5xwB5WMgsgDHsi_0dUeL62uWAnqDQtoBoaR7lj8cI/edit#gid=sharing SiN 300nm Thickness uniformity 2021]
  
 
==SiO<sub>2</sub> deposition (PECVD #1)==
 
==SiO<sub>2</sub> deposition (PECVD #1)==
 
+
*[https://docs.google.com/spreadsheets/d/1uqpg3sirsRbXdTFlxZ6_k3t0ovP0MtpFtICjpH0-prs/edit#gid= SiO2 Standard Recipe]
*[//wiki.nanotech.ucsb.edu/wiki/images/8/87/New_PECVD1-SiN-standard_recipe_2014_SiN_standard_recipe.pdf SiO<sub>2</sub> Standard Recipe (update his page)]
 
*[https://docs.google.com/spreadsheets/d/10ccfgCf5O0JM6L9J5XDz-gWVQz9P24VU/edit#gid= SiO2 Recipe parameters]  
 
  
 
==== Historical Data ====
 
==== Historical Data ====
Line 55: Line 55:
 
*[https://docs.google.com/spreadsheets/d/1DdjIRGsfJ7WCrxQoGpmzkjLGJhpBTFNYLFmmHcNjAjk/edit#gid=sharing SiO<sub>2</sub> 300nm Data 2018]
 
*[https://docs.google.com/spreadsheets/d/1DdjIRGsfJ7WCrxQoGpmzkjLGJhpBTFNYLFmmHcNjAjk/edit#gid=sharing SiO<sub>2</sub> 300nm Data 2018]
 
*[https://docs.google.com/spreadsheets/d/1QbhukSuVNueT067IVEpweSlD4B7GQecf-tfQFQeV6Xs/edit#gid=sharing SiO<sub>2</sub> 300nm Data 2019]
 
*[https://docs.google.com/spreadsheets/d/1QbhukSuVNueT067IVEpweSlD4B7GQecf-tfQFQeV6Xs/edit#gid=sharing SiO<sub>2</sub> 300nm Data 2019]
*[https://docs.google.com/spreadsheets/d/1oVx2Fx7kZA_h4J1L0SMnT4PGWIuuJu5vAfN1JmPzlwc/edit#gid=sharing SiO<sub>2</sub> 300nm Data 2020]
+
*[https://docs.google.com/spreadsheets/d/1OwyhfFPDH-XLPczA8cKoBPnujq9oNukaWkHq0KoFS40/edit#gid=sharing SiO<sub>2</sub> 300nm Data 2020]
 +
*[https://docs.google.com/spreadsheets/d/1I-0Ih_F9pWeOwXeEQC6IFYKNB6bBLSoBiyX8Eu3pwFg/edit#gid=sharing SiO<sub>2</sub> 300nm Data 2021]
 +
 
 +
===== Thick-Film Properties =====
 +
*[https://docs.google.com/spreadsheets/d/1XgUlCaCv3jCK9RyrI553PkIS0PmiAlbWjsDwK5TOH3I/edit#gid=sharing SiO<sub>2</sub> Thick film Data 2021]
  
 
==== Uniformity Data ====
 
==== Uniformity Data ====
Line 66: Line 70:
 
*[https://docs.google.com/spreadsheets/d/1YB_9USpuXGpIdSW2gNsptu5nSrLWAGsYu0SWoYEy0aQ/edit#gid=sharing SiO<sub>2</sub> 300nm Thickness uniformity 2018]
 
*[https://docs.google.com/spreadsheets/d/1YB_9USpuXGpIdSW2gNsptu5nSrLWAGsYu0SWoYEy0aQ/edit#gid=sharing SiO<sub>2</sub> 300nm Thickness uniformity 2018]
 
*[https://docs.google.com/spreadsheets/d/1FatUAEegWuDRzVa47L1_cqgRs0AZ_Fao9jpwz5sfln0/edit#gid=sharing SiO<sub>2</sub> 300nm Thickness uniformity 2019]
 
*[https://docs.google.com/spreadsheets/d/1FatUAEegWuDRzVa47L1_cqgRs0AZ_Fao9jpwz5sfln0/edit#gid=sharing SiO<sub>2</sub> 300nm Thickness uniformity 2019]
*[https://docs.google.com/spreadsheets/d/1cUIEs2_RYK741CAaVVlfzqTEOqlPHQ9MnhgJ6fdTWMc/edit#gid=sharing SiO<sub>2</sub> 300nm Thickness uniformity 2020]
+
*[https://docs.google.com/spreadsheets/d/1uAIEv_z2TJtY2XxTYnDIyKwKT4ZIhalTCyZ5SrDRJmA/edit#gid=sharing SiO<sub>2</sub> 300nm Thickness uniformity 2020]
 +
*[https://docs.google.com/spreadsheets/d/1jThamYtEiH3lVz4IzoG9ILxBG8-TufIKnUd8V0qKQU0/edit#gid=sharing SiO<sub>2</sub> 300nm Thickness uniformity 2021]
  
 
== Low-Stress SiN - LS-SiN (PECVD#1) ==
 
== Low-Stress SiN - LS-SiN (PECVD#1) ==
Line 83: Line 88:
 
The cleaning procedure is very important in order to have consistent result on this tool and also to keep particulate count low. After each deposition you should clean the tool following instructions carefully. The clean is done in two steps:   
 
The cleaning procedure is very important in order to have consistent result on this tool and also to keep particulate count low. After each deposition you should clean the tool following instructions carefully. The clean is done in two steps:   
 
# Wet cleaning (start cleaning by using a cleanroom wipe sprayed with DI. Wipe chamber sidewalls with it. Finish cleaning by using the cleanroom wipe sprayed with IPA. )  
 
# Wet cleaning (start cleaning by using a cleanroom wipe sprayed with DI. Wipe chamber sidewalls with it. Finish cleaning by using the cleanroom wipe sprayed with IPA. )  
# Load the recipe for cleaning " CF4/O2 Clean" (edit the recipe and change ONLY time of cleaning). Follow instructions regarding a required time for cleaning.  
+
# Load the recipe for cleaning "CF4/O2 Clean" (edit the recipe and change ONLY time of cleaning). Follow instructions regarding a required time for cleaning.  
  
=== " CF4/O2 Clean recipe" ===
+
=== [//wiki.nanotech.ucsb.edu/w/images/7/72/PECVD1-cleaning.png Standard Cleaning Recipe: "CF4/O2 Clean"] ===
[[File:PECVD1-cleaning.png|none|thumb|701x701px|PECVD1- cleaning recipe]]
+
Click the above link for a screenshot of the standard cleaning recipe, for which you will enter a custom time. The recipe is set up so that it will '''pop up a window for the cleaning time upon running the recipe''' - you do not need to edit the recipe before running it.
  
 
=[[PECVD 2 (Advanced Vacuum)]]=
 
=[[PECVD 2 (Advanced Vacuum)]]=
Line 100: Line 105:
 
*[https://docs.google.com/spreadsheets/d/1OPZXe8g3H0wywIrPFel3nSZ5iyPs2mVIYUSVKfTtMDg/edit#gid=sharing Particulates in PECVD#2 films 2019]
 
*[https://docs.google.com/spreadsheets/d/1OPZXe8g3H0wywIrPFel3nSZ5iyPs2mVIYUSVKfTtMDg/edit#gid=sharing Particulates in PECVD#2 films 2019]
 
*[https://docs.google.com/spreadsheets/d/1Y9lomsf7bDojeXoAsEG7xvypx_sw_atpmPwB9xtK1Zk/edit#gid=sharing Particulates in PECVD#2 films 2020]
 
*[https://docs.google.com/spreadsheets/d/1Y9lomsf7bDojeXoAsEG7xvypx_sw_atpmPwB9xtK1Zk/edit#gid=sharing Particulates in PECVD#2 films 2020]
 +
*[https://docs.google.com/spreadsheets/d/1BauS7q_sGKkaeY6o3BOw2wyQsyS_DukJxCAbGantDW4/edit#gid=sharing Particulates in PECVD#2 films 2021]
  
 
==SiO<sub>2</sub> deposition (PECVD #2)==
 
==SiO<sub>2</sub> deposition (PECVD #2)==
Line 105: Line 111:
 
==== Standard Recipe ====
 
==== Standard Recipe ====
  
*[https://docs.google.com/spreadsheets/d/1vgWUtpCWC_TFffU9kuR3wqvjryiNA5OV/edit#gid= STD SiO2 Recipe Parameters]
+
 
 
*[https://docs.google.com/spreadsheets/d/1wCEcFj6ZMHR4QifngLXwz6dqbyf8hsVKu7bQbMS6EoA/edit#gid= STD SiO2 Recipe]
 
*[https://docs.google.com/spreadsheets/d/1wCEcFj6ZMHR4QifngLXwz6dqbyf8hsVKu7bQbMS6EoA/edit#gid= STD SiO2 Recipe]
  
Line 118: Line 124:
 
*[https://docs.google.com/spreadsheets/d/1VI-sUmaqois0NsCvf2kQmPfRRa03MjBzl779hmmLtP4/edit#gid=sharing Oxide Data 2018]
 
*[https://docs.google.com/spreadsheets/d/1VI-sUmaqois0NsCvf2kQmPfRRa03MjBzl779hmmLtP4/edit#gid=sharing Oxide Data 2018]
 
*[https://docs.google.com/spreadsheets/d/1oWnQ3D6oknKWU2bohvSrN85rlEZgQN3YP_ZJ4i8u7do/edit#gid=sharing Oxide Data 2019]
 
*[https://docs.google.com/spreadsheets/d/1oWnQ3D6oknKWU2bohvSrN85rlEZgQN3YP_ZJ4i8u7do/edit#gid=sharing Oxide Data 2019]
*[https://docs.google.com/spreadsheets/d/1h5Zrw2hSiMCJrqEsoaRh1lnUVUgKZ67pk-AjmikfrVc/edit#gid=sharing Oxide Data 2020]
+
*[https://docs.google.com/spreadsheets/d/1Z9UMgaQC2PiLLrMk04mpKWkJLa1L_WFMAm5079eKxI0/edit#gid=sharing Oxide Data 2020]
 +
*[https://docs.google.com/spreadsheets/d/10XA3WnHjUZOLFunwUIlM2IqaRIiX_EGb6Jj_bw84gkI/edit#gid=sharing Oxide Data 2021]
 +
 
 +
===== Thin-Film Properties =====
 +
*[https://docs.google.com/spreadsheets/d/19Z8IAVgumWuH0t8RN23LJ2wWZP7jYYLwRl9pDQP4obI/edit#gid=sharing Thick Oxide Data 2021]
  
 
===== Uniformity Data =====
 
===== Uniformity Data =====
Line 128: Line 138:
 
*[https://docs.google.com/spreadsheets/d/1064j6894X63WlRX3Uolxg1q1FRzUZLqSZQA9BWwzPOk/edit#gid=sharing Oxide Thickness Uniformity 2018]
 
*[https://docs.google.com/spreadsheets/d/1064j6894X63WlRX3Uolxg1q1FRzUZLqSZQA9BWwzPOk/edit#gid=sharing Oxide Thickness Uniformity 2018]
 
*[https://docs.google.com/spreadsheets/d/1064j6894X63WlRX3Uolxg1q1FRzUZLqSZQA9BWwzPOk/edit#gid=sharing Oxide Thickness Uniformity 2019]
 
*[https://docs.google.com/spreadsheets/d/1064j6894X63WlRX3Uolxg1q1FRzUZLqSZQA9BWwzPOk/edit#gid=sharing Oxide Thickness Uniformity 2019]
*[https://docs.google.com/spreadsheets/d/1Dx2sNMB9VQQil85SKfnZZ_zqUt1pESfgZeXt3Z3HXJc/edit#gid=sharing Oxide Thickness Uniformity 2020]
+
*[https://docs.google.com/spreadsheets/d/1Z9UMgaQC2PiLLrMk04mpKWkJLa1L_WFMAm5079eKxI0/edit#gid=sharing Oxide Thickness Uniformity 2020]
 +
*[https://docs.google.com/spreadsheets/d/1b9Fmzp_d-XiMerFtrDiCsmS7NMNoaBtS8T0DLqoii8Y/edit#gid=sharing Oxide Thickness Uniformity 2021]
  
 
==SiN deposition (PECVD #2)==
 
==SiN deposition (PECVD #2)==
Line 135: Line 146:
  
 
*[//wiki.nanotech.ucsb.edu/wiki/images/4/4c/SiNx_Films_by_PECVD2.pdf SiNx Film Stress vs LF and HF Duration Time, and Gas Flowing-rate]
 
*[//wiki.nanotech.ucsb.edu/wiki/images/4/4c/SiNx_Films_by_PECVD2.pdf SiNx Film Stress vs LF and HF Duration Time, and Gas Flowing-rate]
*[https://docs.google.com/spreadsheets/d/1Oegk0aFFCuz9wQHDN2Kdz0NFo9_wuEVW/edit?dls=true#gid= STD Nitride2 Recipe Parameters]
 
 
 
*[https://docs.google.com/spreadsheets/d/1KS4HfhUJyYVep4H6CRAKpMRP5TA31F0qD-obQkKRnEI/edit#gid= STD Nitride2 Recipe]
 
*[https://docs.google.com/spreadsheets/d/1KS4HfhUJyYVep4H6CRAKpMRP5TA31F0qD-obQkKRnEI/edit#gid= STD Nitride2 Recipe]
  
Line 149: Line 158:
 
*[https://docs.google.com/spreadsheets/d/1OO0ewGSqYSzL3lj8fXkgckTkBGQRliD6sBc02IW7wZY/edit#gid=sharing Nitride2 Data 2018]
 
*[https://docs.google.com/spreadsheets/d/1OO0ewGSqYSzL3lj8fXkgckTkBGQRliD6sBc02IW7wZY/edit#gid=sharing Nitride2 Data 2018]
 
*[https://docs.google.com/spreadsheets/d/1Zi8CRspd3LTDdNRRCneE0--bVohWvZbV_kSHo04s0oI/edit#gid=sharing Nitride2 Data 2019]
 
*[https://docs.google.com/spreadsheets/d/1Zi8CRspd3LTDdNRRCneE0--bVohWvZbV_kSHo04s0oI/edit#gid=sharing Nitride2 Data 2019]
*[https://docs.google.com/spreadsheets/d/1T0Zk2geshX9h-Cf8I1BAcQqWFhCqorJrrOnDH4hz7GY/edit#gid=sharing Nitride2 Data 2020]
+
*[https://docs.google.com/spreadsheets/d/1LEutQynQXU_9B4EqRt21PX9TGR13IqaMge7sKAXKAfg/edit#gid=sharing Nitride2 Data 2020]
 +
*[https://docs.google.com/spreadsheets/d/1piGMPEHXiUV5WMNfaTFKdL1pnE8W2yrWHkNWHd7Au1A/edit#gid=sharing Nitride2 Data 2021]
  
 
===== Uniformity Data =====
 
===== Uniformity Data =====
Line 159: Line 169:
 
*[https://docs.google.com/spreadsheets/d/1hzj4Fb5fN8lS0m9-rm9AgEn0Zunif5grI4X7YkAMEFU/edit#gid=sharing Nitride2 Thickness Uniformity 2018]
 
*[https://docs.google.com/spreadsheets/d/1hzj4Fb5fN8lS0m9-rm9AgEn0Zunif5grI4X7YkAMEFU/edit#gid=sharing Nitride2 Thickness Uniformity 2018]
 
*[https://docs.google.com/spreadsheets/d/1hzj4Fb5fN8lS0m9-rm9AgEn0Zunif5grI4X7YkAMEFU/edit#gid=sharing Nitride2 Thickness Uniformity 2019]
 
*[https://docs.google.com/spreadsheets/d/1hzj4Fb5fN8lS0m9-rm9AgEn0Zunif5grI4X7YkAMEFU/edit#gid=sharing Nitride2 Thickness Uniformity 2019]
*[https://docs.google.com/spreadsheets/d/16nlLjk_kctE6YKQBJbq0SotP80tybdSdJ0hvxbeohE0/edit#gid=sharing Nitride2 Thickness Uniformity 2020]
+
*[https://docs.google.com/spreadsheets/d/1xdzjLODpe2Xb7r4PGil1q-OFqSYKuZBivqLt1T6lezw/edit#gid=sharing Nitride2 Thickness Uniformity 2020]
 +
*[https://docs.google.com/spreadsheets/d/19x70-CIyQ41pywpL-IusldLv7XYJps9aJT5-rYYQSCs/edit#gid=sharing Nitride2 Thickness Uniformity 2021]
  
 
==Low-Stress SiN deposition (PECVD #2)==
 
==Low-Stress SiN deposition (PECVD #2)==
Line 166: Line 177:
 
==== Standard Recipe ====
 
==== Standard Recipe ====
  
*[https://docs.google.com/spreadsheets/d/1qXCH1phgvk3-5_5FUqeQaGPERhyS5dn4/edit#gid= STD LS Nitride2 Recipe Parameters]
 
 
*[https://docs.google.com/spreadsheets/d/1DzzI7aE61R7c6gyk6cGBdm9FtGrApiNJ4AL90ll2C8k/edit#gid= STD LS Nitride2 Recipe]
 
*[https://docs.google.com/spreadsheets/d/1DzzI7aE61R7c6gyk6cGBdm9FtGrApiNJ4AL90ll2C8k/edit#gid= STD LS Nitride2 Recipe]
 
*''Old Versions:''
 
*''Old Versions:''
Line 182: Line 192:
 
*[https://docs.google.com/spreadsheets/d/1vwpDtiglR2DLWiYNhpBX77cyyj9lw55iVeFz1puN7bM/edit#gid=sharing LS Nitride2 Data 2018]
 
*[https://docs.google.com/spreadsheets/d/1vwpDtiglR2DLWiYNhpBX77cyyj9lw55iVeFz1puN7bM/edit#gid=sharing LS Nitride2 Data 2018]
 
*[https://docs.google.com/spreadsheets/d/1zvSl2P5T926Ol48yH3FBCZm1zCeycl3S8GWQYtzi8VI/edit#gid=sharing LS Nitride2 Data 2019]
 
*[https://docs.google.com/spreadsheets/d/1zvSl2P5T926Ol48yH3FBCZm1zCeycl3S8GWQYtzi8VI/edit#gid=sharing LS Nitride2 Data 2019]
*[https://docs.google.com/spreadsheets/d/1SxW4t3xkiSkEPobUkpPF9m_gcC6yiaOPRlIgCWyqebg/edit#gid=sharing LS Nitride2 Data 2020]
+
*[https://docs.google.com/spreadsheets/d/1muyFsIspqZXB2HXiqG3t39uzeO7A7Srvh4aGdXjwCc4/edit#gid=sharing LS Nitride2 Data 2020]
 +
*[https://docs.google.com/spreadsheets/d/1qzVA44esh71655lE1rrpGkKKNTyZRC_mv3IaiZ_HAWQ/edit#gid=sharing LS Nitride2 Data 2021]
  
 
===== Uniformity Data =====
 
===== Uniformity Data =====
Line 192: Line 203:
 
*[https://docs.google.com/spreadsheets/d/17OGrhbvP8O_0mBMIsmUmEwfyFaoJnNNpMFpgBUW7qzI/edit#gid=sharing LS Nitride2 Thickness Uniformity 2018]
 
*[https://docs.google.com/spreadsheets/d/17OGrhbvP8O_0mBMIsmUmEwfyFaoJnNNpMFpgBUW7qzI/edit#gid=sharing LS Nitride2 Thickness Uniformity 2018]
 
*[https://docs.google.com/spreadsheets/d/17OGrhbvP8O_0mBMIsmUmEwfyFaoJnNNpMFpgBUW7qzI/edit#gid=sharing LS Nitride2 Thickness Uniformity 2019]
 
*[https://docs.google.com/spreadsheets/d/17OGrhbvP8O_0mBMIsmUmEwfyFaoJnNNpMFpgBUW7qzI/edit#gid=sharing LS Nitride2 Thickness Uniformity 2019]
*[https://docs.google.com/spreadsheets/d/1TMasE4I--H948aKCWEO1Y3Dw2pCA6-iqQ0km3v_2VFo/edit#gid=sharing LS Nitride2 Thickness Uniformity 2020]
+
*[https://docs.google.com/spreadsheets/d/1M4ug8SAqy2Ky70LNLW3pL2MjSs69beJVhbC2BbabHaU/edit#gid=sharing LS Nitride2 Thickness Uniformity 2020]
 +
*[https://docs.google.com/spreadsheets/d/12wvXFHN7CV_XSFj6hB5Gd7SIXERwzkTM__58ZqzPOuk/edit#gid=sharing LS Nitride2 Thickness Uniformity 2021]
  
 
==Amorphous-Si deposition (PECVD #2)==
 
==Amorphous-Si deposition (PECVD #2)==
Line 202: Line 214:
 
The cleaning procedure is very important in order to have consistent result on this tool and also to keep particulate count low. After each deposition you should clean the tool following instructions carefully. The clean is done in two steps:
 
The cleaning procedure is very important in order to have consistent result on this tool and also to keep particulate count low. After each deposition you should clean the tool following instructions carefully. The clean is done in two steps:
 
#Wet cleaning (start cleaning by using a cleanroom wipe sprayed with DI. Wipe chamber sidewalls with it. Finish cleaning by using the cleanroom wipe sprayed with IPA. )
 
#Wet cleaning (start cleaning by using a cleanroom wipe sprayed with DI. Wipe chamber sidewalls with it. Finish cleaning by using the cleanroom wipe sprayed with IPA. )
#Load the recipe for cleaning " STD CF4/O2 Clean" (edit the recipe and change ONLY time of cleaning). Follow instructions regarding a required time for cleaning.
+
#Load the recipe for cleaning "STD CF4/O2 Clean" (edit the recipe and change ONLY time of cleaning). Follow instructions regarding a required time for cleaning.
===" STD CF4/O2 Clean recipe" ===
+
===[//wiki.nanotech.ucsb.edu/w/images/3/34/PECVD2_photo_for_cleaning.png Standard Clean Recipe: "STD CF4/O2 Clean recipe"] ===
[[File:PECVD2 photo for cleaning.png|none|thumb|725x725px|Advanced PECVD2 Cleaning recipe]]
+
Click the above link for a screenshot of the standard cleaning recipe, for which you will enter a custom time. The recipe is set up so that it will '''pop up a window for the cleaning time upon running the recipe''' - you do not need to edit the recipe before running it.
  
 
=[[ICP-PECVD (Unaxis VLR)]]=
 
=[[ICP-PECVD (Unaxis VLR)]]=
 +
2020-02: New recipes have been characterized for low particulate count and repeatability.  Only staff-supplied recipes are allowed in the tool. Please follow the [[ICP-PECVD (Unaxis VLR)#Documentation|'''new procedures''']] to ensure low particle counts in the chamber.
  
 +
The system currently has '''Deuterated Silane (SiD<sub>4</sub>) installed''' - identical to the regular Silicon precursor SiH<sub>4</sub>, except that it significantly lowers optical absorption in the near-infrared due to shifted molecular vibrations/molecular weights.
  
 
==== Historical Particulate Data ====
 
==== Historical Particulate Data ====
Line 213: Line 227:
 
* [https://docs.google.com/spreadsheets/d/1fMebt-6BfAurcjMv1aDsmm6VgPqokU73_2ReZFqzEEk/edit#gid=sharing Particulates in Unaxis films @250C-2020]
 
* [https://docs.google.com/spreadsheets/d/1fMebt-6BfAurcjMv1aDsmm6VgPqokU73_2ReZFqzEEk/edit#gid=sharing Particulates in Unaxis films @250C-2020]
  
 
+
==== Standard Recipes ====
==== Sandard Recipes ====
+
*[https://docs.google.com/spreadsheets/d/1T_4gaJQ3wHSNptoAtFR1fN0ePwfw3PsQ0DLSjqGeyM4/edit#gid=sharing SiO2 LDR 250C Recipe-2020]
 +
*[https://docs.google.com/spreadsheets/d/1nsdGPpfyZfIesyYG1PIU9uYyuzQWrfpsvVWM6J_H6BI/edit#gid=sharing SiO2 HDR 250C Recipe-2020]
 
*[https://docs.google.com/spreadsheets/d/1UTr93aWx0MjCwVBwRmYjPwo9ASluGQ-OrJhVG_R57aY/edit#gid=sharing SiN 250C Recipe-2020]
 
*[https://docs.google.com/spreadsheets/d/1UTr93aWx0MjCwVBwRmYjPwo9ASluGQ-OrJhVG_R57aY/edit#gid=sharing SiN 250C Recipe-2020]
 
*[https://docs.google.com/spreadsheets/d/1MXW7UNpTyk93ucOVQaSun5IX7QaUbSABNHNznb09qw8/edit#gid=sharing SiN LS 250C Recipe-2020]
 
*[https://docs.google.com/spreadsheets/d/1MXW7UNpTyk93ucOVQaSun5IX7QaUbSABNHNznb09qw8/edit#gid=sharing SiN LS 250C Recipe-2020]
*[https://docs.google.com/spreadsheets/d/1T_4gaJQ3wHSNptoAtFR1fN0ePwfw3PsQ0DLSjqGeyM4/edit#gid=sharing SiO2 LDR 250C Recipe-2020]
 
*[https://docs.google.com/spreadsheets/d/1nsdGPpfyZfIesyYG1PIU9uYyuzQWrfpsvVWM6J_H6BI/edit#gid=sharing SiO2 HDR 250C Recipe-2020]
 
 
  
== SiN 250C deposition (Unaxis VLR) ==
+
==SiO2 LDR 250C Deposition (Unaxis VLR)==
 +
''Low-Deposition Rate SiO<sub>2</sub>''
  
 
==== Historical Data ====
 
==== Historical Data ====
 +
===== Thin-Film Properties =====
 +
This data is for 780sec long SiO2 LDR (low deposition rate) deposition, and cleaning time is 900sec, following the procedure [[here]].
 +
*[https://docs.google.com/spreadsheets/d/1wocoCPOOEDQcZbXJJNaZs1sr9dXBZpn1wUyglL8IQrI/edit#gid=sharing SiO2 LDR 250C 300nm Data-2019]
 +
*[https://docs.google.com/spreadsheets/d/1bU2Gu3x3DNyrq8skMAQZJCsra-IcoDCT0U5D135YPgc/edit#gid=sharing SiO2 LDR 250C 300nm Data-2020]
 +
===== Uniformity Data =====
 +
*[https://docs.google.com/spreadsheets/d/1Xi21OrargcNRthZ2fM_56APB8O599ctDfq5E_6B5Ft0/edit#gid=sharing Thickness Uniformity SiO2 LDR 250C 300nm-2019]
 +
*[https://docs.google.com/spreadsheets/d/1-ytu5R75FAXNfhJZTRuK2eRZyu_L6Hy1BWV2zN6_tRA/edit#gid=sharing Thickness Uniformity SiO2 LDR 250C 300nm-2020]
  
 +
==SiO2 HDR 250C Deposition (Unaxis VLR)==
 +
''High-Deposition Rate SiO<sub>2</sub>''
  
 +
==== Historical Data ====
 
===== Thin-Film Properties =====
 
===== Thin-Film Properties =====
 +
This data is for 180sec long SiO2 HDR ( high deposition rate) deposition, and cleaning time is 900sec, following the procedure [[here]].
 +
*[https://docs.google.com/spreadsheets/d/16s-tUna9xrkKneK1lE-qSPuUHWlDmP6Qu3IngBXP3R8/edit#gid=sharing SiO2 HDR 250C 300nm Data-2019]
 +
*[https://docs.google.com/spreadsheets/d/1OxHi5r9ifNvF8ODpIk6aoRevb4RdbbykwPVMm1g-yi4/edit#gid=sharing SiO2 HDR 250C 300nm Data-2020]
 +
===== Uniformity Data =====
 +
*[https://docs.google.com/spreadsheets/d/1Mm_rsTm9xDQ50kZx6X6EZ5dTegUvinq0zFxRtE8B2R4/edit#gid=sharing Thickness Uniformity SiO2 HDR 250C 300nm-2019]
 +
*[https://docs.google.com/spreadsheets/d/1nzVeCKsmgL17zft6axQlixpvsEowJOG7qCnLQm_0XxE/edit#gid=sharing Thickness Uniformity SiO2 HDR 250C 300nm-2020]
  
 +
== SiN 250C deposition (Unaxis VLR) ==
 +
==== Historical Data ====
 +
===== Thin-Film Properties =====
 +
This data is for 480sec long SiN deposition, and cleaning time is 1500sec, following the procedure [[here]].
 
*[https://docs.google.com/spreadsheets/d/1VrgS0cB2OcdZVTCnDAesgQCLRaAgEB_Iajc_OrhXOo0/edit#gid=sharing SiN 250C 300nm Data-2020]
 
*[https://docs.google.com/spreadsheets/d/1VrgS0cB2OcdZVTCnDAesgQCLRaAgEB_Iajc_OrhXOo0/edit#gid=sharing SiN 250C 300nm Data-2020]
 
 
===== Uniformity Data =====
 
===== Uniformity Data =====
 
*[https://docs.google.com/spreadsheets/d/1YAx_Ix84xId8CAhDwZeFT7jLFUwg-BET9aBwg3DxUmQ/edit#gid=sharing Thickness Uniformity SiN 250C 300nm-2020]
 
*[https://docs.google.com/spreadsheets/d/1YAx_Ix84xId8CAhDwZeFT7jLFUwg-BET9aBwg3DxUmQ/edit#gid=sharing Thickness Uniformity SiN 250C 300nm-2020]
  
 +
== SiN LS 250C Deposition (Unaxis VLR) ==
 +
''Low Stress Silicon-Nitride''
  
== SiN LS 250C Deposition (Unaxis VLR) ==
+
==== Historical Data ====
 +
''To Be Added''
  
=== Thin-Film Properties ===
+
===== Thin-Film Properties =====
 +
This data is for 180sec long SiN LS (low stress) deposition, and cleaning time is 1500sec, following the procedure [[here]].
 
*[https://docs.google.com/spreadsheets/d/1i2mE2K12EEulnCbO9KuU9PCcvHAmcGxTIXUF8x4IOWk/edit#gid=sharing SiN LS 250C 300nm Data-2020]
 
*[https://docs.google.com/spreadsheets/d/1i2mE2K12EEulnCbO9KuU9PCcvHAmcGxTIXUF8x4IOWk/edit#gid=sharing SiN LS 250C 300nm Data-2020]
 
+
===== Uniformity Data =====
=== Uniformity Data ===
 
 
*[https://docs.google.com/spreadsheets/d/1NDyxH1i9COM2XTryLqYPE9yOekgRslAJUO7o56iTOEQ/edit#gid=sharing Thickness Uniformity SiN LS 250C 300nm-2020]
 
*[https://docs.google.com/spreadsheets/d/1NDyxH1i9COM2XTryLqYPE9yOekgRslAJUO7o56iTOEQ/edit#gid=sharing Thickness Uniformity SiN LS 250C 300nm-2020]
 
==SiO2 250C Deposition (Unaxis VLR)==
 
 
=== Thin-Film Properties ===
 
 
*[https://docs.google.com/spreadsheets/d/1wocoCPOOEDQcZbXJJNaZs1sr9dXBZpn1wUyglL8IQrI/edit#gid=sharing SiO2 LDR 250C 300nm Data-2019]
 
*[https://docs.google.com/spreadsheets/d/1bU2Gu3x3DNyrq8skMAQZJCsra-IcoDCT0U5D135YPgc/edit#gid=sharing SiO2 LDR 250C 300nm Data-2020]
 
*[https://docs.google.com/spreadsheets/d/16s-tUna9xrkKneK1lE-qSPuUHWlDmP6Qu3IngBXP3R8/edit#gid=sharing SiO2 HDR 250C 300nm Data-2019]
 
*[https://docs.google.com/spreadsheets/d/1OxHi5r9ifNvF8ODpIk6aoRevb4RdbbykwPVMm1g-yi4/edit#gid=sharing SiO2 HDR 250C 300nm Data-2020]
 
 
=== Uniformity Data ===
 
 
*[https://docs.google.com/spreadsheets/d/1Xi21OrargcNRthZ2fM_56APB8O599ctDfq5E_6B5Ft0/edit#gid=sharing Thickness Uniformity SiO2 LDR 250C 300nm-2019]
 
*[https://docs.google.com/spreadsheets/d/1-ytu5R75FAXNfhJZTRuK2eRZyu_L6Hy1BWV2zN6_tRA/edit#gid=sharing Thickness Uniformity SiO2 LDR 250C 300nm-2020]
 
*[https://docs.google.com/spreadsheets/d/1Mm_rsTm9xDQ50kZx6X6EZ5dTegUvinq0zFxRtE8B2R4/edit#gid=sharing Thickness Uniformity SiO2 HDR 250C 300nm-2019]
 
*[https://docs.google.com/spreadsheets/d/1nzVeCKsmgL17zft6axQlixpvsEowJOG7qCnLQm_0XxE/edit#gid=sharing Thickness Uniformity SiO2 HDR 250C 300nm-2020]
 
  
 
== Cleaning Recipes (Unaxis VLR Dep) ==
 
== Cleaning Recipes (Unaxis VLR Dep) ==
Line 262: Line 281:
 
* SiNx etches at 20nm/min
 
* SiNx etches at 20nm/min
 
* SiO2 etches at 40nm/min
 
* SiO2 etches at 40nm/min
===" Post-Dep Clean" recipe===
 
Add the picture of " Post-Dep Clean" recipe
 

Latest revision as of 15:47, 19 February 2021

Back to Vacuum Deposition Recipes.

PECVD 1 (PlasmaTherm 790)

Historical Particulate Data

SiN deposition (PECVD #1)

Historical Data

Thin-Film Properties
Uniformity Data

SiO2 deposition (PECVD #1)

Historical Data

Thin-Film Properties
Thick-Film Properties

Uniformity Data

Low-Stress SiN - LS-SiN (PECVD#1)

SiOxNy deposition (PECVD #1)

Cleaning Recipes (PECVD #1)

The cleaning procedure is very important in order to have consistent result on this tool and also to keep particulate count low. After each deposition you should clean the tool following instructions carefully. The clean is done in two steps:

  1. Wet cleaning (start cleaning by using a cleanroom wipe sprayed with DI. Wipe chamber sidewalls with it. Finish cleaning by using the cleanroom wipe sprayed with IPA. )
  2. Load the recipe for cleaning "CF4/O2 Clean" (edit the recipe and change ONLY time of cleaning). Follow instructions regarding a required time for cleaning.

Standard Cleaning Recipe: "CF4/O2 Clean"

Click the above link for a screenshot of the standard cleaning recipe, for which you will enter a custom time. The recipe is set up so that it will pop up a window for the cleaning time upon running the recipe - you do not need to edit the recipe before running it.

PECVD 2 (Advanced Vacuum)

Historical Particulate Data

SiO2 deposition (PECVD #2)

Standard Recipe

Historical Data

Thin-Film Properties
Thin-Film Properties
Uniformity Data

SiN deposition (PECVD #2)

Standard Recipe

Historical Data

Thin-Film Properties
Uniformity Data

Low-Stress SiN deposition (PECVD #2)

Low-Stress SilIcon Nitride (< 100 MPa)

Standard Recipe

Historical Data

Thin-Film Properties
Uniformity Data

Amorphous-Si deposition (PECVD #2)

Cleaning Recipes (PECVD #2)

The cleaning procedure is very important in order to have consistent result on this tool and also to keep particulate count low. After each deposition you should clean the tool following instructions carefully. The clean is done in two steps:

  1. Wet cleaning (start cleaning by using a cleanroom wipe sprayed with DI. Wipe chamber sidewalls with it. Finish cleaning by using the cleanroom wipe sprayed with IPA. )
  2. Load the recipe for cleaning "STD CF4/O2 Clean" (edit the recipe and change ONLY time of cleaning). Follow instructions regarding a required time for cleaning.

Standard Clean Recipe: "STD CF4/O2 Clean recipe"

Click the above link for a screenshot of the standard cleaning recipe, for which you will enter a custom time. The recipe is set up so that it will pop up a window for the cleaning time upon running the recipe - you do not need to edit the recipe before running it.

ICP-PECVD (Unaxis VLR)

2020-02: New recipes have been characterized for low particulate count and repeatability.  Only staff-supplied recipes are allowed in the tool. Please follow the new procedures to ensure low particle counts in the chamber.
The system currently has Deuterated Silane (SiD4) installed - identical to the regular Silicon precursor SiH4, except that it significantly lowers optical absorption in the near-infrared due to shifted molecular vibrations/molecular weights.

Historical Particulate Data

Standard Recipes

SiO2 LDR 250C Deposition (Unaxis VLR)

Low-Deposition Rate SiO2

Historical Data

Thin-Film Properties

This data is for 780sec long SiO2 LDR (low deposition rate) deposition, and cleaning time is 900sec, following the procedure here.

Uniformity Data

SiO2 HDR 250C Deposition (Unaxis VLR)

High-Deposition Rate SiO2

Historical Data

Thin-Film Properties

This data is for 180sec long SiO2 HDR ( high deposition rate) deposition, and cleaning time is 900sec, following the procedure here.

Uniformity Data

SiN 250C deposition (Unaxis VLR)

Historical Data

Thin-Film Properties

This data is for 480sec long SiN deposition, and cleaning time is 1500sec, following the procedure here.

Uniformity Data

SiN LS 250C Deposition (Unaxis VLR)

Low Stress Silicon-Nitride

Historical Data

To Be Added

Thin-Film Properties

This data is for 180sec long SiN LS (low stress) deposition, and cleaning time is 1500sec, following the procedure here.

Uniformity Data

Cleaning Recipes (Unaxis VLR Dep)

You must edit the Post-Dep Clean recipe to correspond to your deposited thickness and material. See the Operating Procedure on the Unaxis Tool Page for details.

  • SiNx etches at 20nm/min
  • SiO2 etches at 40nm/min