Difference between revisions of "PECVD1 Wafer Coating Process"
Jump to navigation
Jump to search
(corrected titles) |
|||
(2 intermediate revisions by one other user not shown) | |||
Line 1: | Line 1: | ||
− | There are two standard recipes for SiN and SiO2 at 250C in PECVD#1. Instructions bellow explain how to run |
+ | There are two standard recipes for SiN and SiO2 deposition at 250C in PECVD#1. Instructions bellow explain how to run process (seasoning, deposition, cleaning). |
− | === |
+ | === Standard Si3N4 (Silicon-Nitride) Deposition === |
− | ==== SiN |
+ | ==== SiN Deposition ==== |
# Log in to PECVD #1 |
# Log in to PECVD #1 |
||
# Seasoning |
# Seasoning |
||
Line 17: | Line 17: | ||
#* Log out |
#* Log out |
||
− | === SiO2 |
+ | === Standard Oxide, SiO2 (Silicon Dioxide) Deposition === |
+ | |||
+ | ==== SiO2 Deposition ==== |
||
#Log in to PECVD #1 |
#Log in to PECVD #1 |
||
# Seasoning |
# Seasoning |
Latest revision as of 13:16, 10 December 2020
There are two standard recipes for SiN and SiO2 deposition at 250C in PECVD#1. Instructions bellow explain how to run process (seasoning, deposition, cleaning).
Standard Si3N4 (Silicon-Nitride) Deposition
SiN Deposition
- Log in to PECVD #1
- Seasoning
- Load the seasoning recipe (SiN seasoning), and run it. The goal of this step is to coat chamber walls and prepare it for deposition.
- Deposition
- Vent the chamber and load the substrate (place it in the center of platen). You can place small pieces around the wafer to protect it from moving.
- Pump down.
- Load the deposition recipe (SiN@250C), and run it. Deposition time is variable. Get the rate from historical data.
- Unload the wafer.
- Cleaning
- Wipe sidewall first with DI water, followed by IPA.
- Load the cleaning recipe (CH4/O2 clean). Edit the recipe and enter required time for cleaning.
- Log out
Standard Oxide, SiO2 (Silicon Dioxide) Deposition
SiO2 Deposition
- Log in to PECVD #1
- Seasoning
- Load the seasoning recipe( SiO2 seasoning), and run it. The goal of this step is to coat chamber walls and prepare it for deposition.
- Deposition
- Vent the chamber and load the substarte (place it in the center of platen). You can place small pieces around the wafer to protect it from moving.
- Pump down.
- Load the deposition recipe( SiO2@250C), and run it. Deposition time is variable. Get the rate from historical data.
- Unload the wafer.
- Cleaning
- Wipe sidewall first with DI water, followed by IPA.
- Load for cleaning recipe (CF4/O2). Edit the recipe and enter required time for cleaning.
- Log out