Difference between revisions of "PECVD1 Wafer Coating Process"

From UCSB Nanofab Wiki
Jump to navigation Jump to search
(SiN and SiO2 depositions)
(corrected titles)
 
(One intermediate revision by one other user not shown)
Line 1: Line 1:
 
There are two standard recipes for SiN and SiO2 deposition at 250C in PECVD#1. Instructions bellow explain how to run process (seasoning, deposition, cleaning).
 
There are two standard recipes for SiN and SiO2 deposition at 250C in PECVD#1. Instructions bellow explain how to run process (seasoning, deposition, cleaning).
   
  +
=== Standard Si3N4 (Silicon-Nitride) Deposition ===
=== PECVD#1 ===
 
   
==== SiN deposition ====
+
==== SiN Deposition ====
 
# Log in to PECVD #1
 
# Log in to PECVD #1
 
# Seasoning
 
# Seasoning
Line 17: Line 17:
 
#* Log out
 
#* Log out
   
=== SiO2 deposition ===
+
=== Standard Oxide, SiO2 (Silicon Dioxide) Deposition ===
  +
  +
==== SiO2 Deposition ====
 
#Log in to PECVD #1
 
#Log in to PECVD #1
 
# Seasoning
 
# Seasoning

Latest revision as of 13:16, 10 December 2020

There are two standard recipes for SiN and SiO2 deposition at 250C in PECVD#1. Instructions bellow explain how to run process (seasoning, deposition, cleaning).

Standard Si3N4 (Silicon-Nitride) Deposition

SiN Deposition

  1. Log in to PECVD #1
  2. Seasoning
    • Load the seasoning recipe (SiN seasoning), and run it. The goal of this step is to coat chamber walls and prepare it for deposition.
  3. Deposition
    • Vent the chamber and load the substrate (place it in the center of platen). You can place small pieces around the wafer to protect it from moving.
    • Pump down.
    • Load the deposition recipe (SiN@250C), and run it. Deposition time is variable. Get the rate from historical data.
    • Unload the wafer.
  4. Cleaning
    • Wipe sidewall first with DI water, followed by IPA.
    • Load the cleaning recipe (CH4/O2 clean). Edit the recipe and enter required time for cleaning.
    • Log out

Standard Oxide, SiO2 (Silicon Dioxide) Deposition

SiO2 Deposition

  1. Log in to PECVD #1
  2. Seasoning
    • Load the seasoning recipe( SiO2 seasoning), and run it. The goal of this step is to coat chamber walls and prepare it for deposition.
  3. Deposition
    • Vent the chamber and load the substarte (place it in the center of platen). You can place small pieces around the wafer to protect it from moving.
    • Pump down.
    • Load the deposition recipe( SiO2@250C), and run it. Deposition time is variable. Get the rate from historical data.
    • Unload the wafer.
  4. Cleaning
    • Wipe sidewall first with DI water, followed by IPA.
    • Load for cleaning recipe (CF4/O2). Edit the recipe and enter required time for cleaning.
    • Log out