+ | [[Table SiO2 recipe]] |
||
− | === PECVD#1 deposition - 300nm SiN film @250°C === |
||
− | The wafers are ordered from SVM. These are low particle count 4" Si wafer where particle count is very low <100. |
||
− | |||
− | a)Log in to PECVD #1 (Staff account) |
||
− | |||
− | b)Edit standard recipes (for seasoning, deposition, and cleaning). You can '''ONLY''' change the time in recipes. |
||
− | * •Seasoning recipe name: |
||
− | * •Deposition recipe name: |
||
− | * •Cleaning recipe name: |
||
− | c)Load the recipe for seasoning, and run it. The goal of this step is to coat chamber walls and prepare it for deposition. |
||
− | |||
− | d)Vent the chamber and load 4"Si wafer (place in in the center of platen). You can place small pieces around, to protect wafer from moving |
||
− | |||
− | e)Pump down and load the recipe for deposition. |
||
− | |||
− | f) Edit the recipe for deposition, change the time ONLY. |
||
− | |||
− | g) Run deposition |
||
− | |||
− | h) Wait for deposition to be finished. Unload the wafer |
||
− | |||
− | i) Wipe sidewall first with water then with IPA. |
||
− | |||
− | j) Load recipe for cleaning. Edit the recipe and enter required time for cleaning. |
||
− | |||
− | === PECVD#1 deposition - 300nm SiO2 film @250°C === |
||
− | The wafers are ordered from SVM. These are low particle count 4" Si wafer where particle count is very low <100. |
||
− | |||
− | a)Log in to PECVD #1 (Staff account) |
||
− | |||
− | b)Edit standard recipes (for seasoning, deposition, and cleaning). You can '''ONLY''' change the time in recipes. |
||
− | * •Seasoning recipe name: |
||
− | * •Deposition recipe name: |
||
− | * •Cleaning recipe name: |
||
− | c)Load the recipe for seasoning, and run it. The goal of this step is to coat chamber walls and prepare it for deposition. |
||
− | |||
− | d)Vent the chamber and load 4"Si wafer (place in in the center of platen). You can place small pieces around, to protect wafer from moving |
||
− | |||
− | e)Pump down and load the recipe for deposition. |
||
− | |||
− | f) Edit the recipe for deposition, change the time ONLY. |
||
− | |||
− | g) Run deposition |
||
− | |||
− | h) Wait for deposition to be finished. Unload the wafer |
||
− | |||
− | i) Wipe sidewall first with water then with IPA. |
||
− | |||
− | j) Load recipe for cleaning. Edit the recipe and enter required time for cleaning. |
||
− | |||
− | k)Run the cleaning recipe. |