Difference between revisions of "Oxford ICP Etcher - Process Control Data"

From UCSB Nanofab Wiki
Jump to navigation Jump to search
m (added new data, also changed units from nm to um)
m (Added etch rate as well as SEMs for 1x1cm pieces)
Line 7: Line 7:
 
|Date
 
|Date
 
|Sample#
 
|Sample#
|Etch  Rate (um/min)
+
|Etch  Rate (nm/min)
 
|Etch  Selectivity (InP/SiO2)
 
|Etch  Selectivity (InP/SiO2)
 
|Comments
 
|Comments
Line 13: Line 13:
 
|-
 
|-
 
|1/26/22
 
|1/26/22
|<small>NP_?</small>
+
|<small>NP_1_26_001</small>
|testing [[Oxford ICP Etcher (PlasmaPro 100 Cobra)#Recipes|link]]
+
|374
 
|
 
|
 
|
 
|
|[https://wiki.nanotech.ucsb.edu/w/images/f/f5/Oxford_InP_Cal_-_SEM_45D_001.jpg <nowiki>[1]</nowiki>]
+
|[https://wiki.nanotech.ucsb.edu/w/images/d/dc/Oxford_Cal_1_26_22_001_45D_005.jpg <nowiki>[1]</nowiki>] [https://wiki.nanotech.ucsb.edu/w/images/8/87/Oxford_Cal_1_26_22_001_CS_004.jpg <nowiki>[2]</nowiki>]
 +
|-
 +
|1/26/22
 +
|NP_1_26_003
 +
|362
 +
|
 +
|Better images will taken soon
 +
|[https://wiki.nanotech.ucsb.edu/w/images/a/a4/Oxford_Cal_1_26_22_003_45D_002.jpg <nowiki>[1]</nowiki>] [https://wiki.nanotech.ucsb.edu/w/images/d/de/Oxford_Cal_1_26_22_003_CS007.jpg <nowiki>[2]</nowiki>]
 
|}
 
|}
  

Revision as of 11:11, 8 February 2022

Data - InP Ridge Etch (Oxford ICP Etcher)

PECVD SiO2 hardmask, patterned on Stepper #2 (AutoStep 200) & Panasonic ICP #1

InP Ridge Etch: 60°C, 3mT, 800W/65W, Cl2=18, H2=15, CH4=10sccm, time=5min00sec (300sec)

Sample Size: 1x1cm, ~30-40% SiO2 masking (NingC's pattern). Silicon carrier, no adhesive.

Date Sample# Etch Rate (nm/min) Etch Selectivity (InP/SiO2) Comments SEM Images
1/26/22 NP_1_26_001 374 [1] [2]
1/26/22 NP_1_26_003 362 Better images will taken soon [1] [2]

Dependence on Sample Size

We have found that the size of the InP piece loaded (no adhesive, onto Silicon carrier wafer) affects the etch rate, but does not affect the etch profile - ie. etches are still smooth and vertical, but rate varies with sample area.

InP Ridge Etch: 60°C, 3mT, 800W/65W, Cl2=18, H2=15, CH4=10sccm, time=5min05sec (305sec)

Silicon carrier, no adhesive.

Date Sample# Sample Size (dimensions, mm) Sample Size (area, mm2) Etch Rate (um/min) Etch Selectivity (InP/SiO2) Comments SEM Images
1/11/22 DJ_InPRidge 4.5 x 2.5 11.25 0.602 64.6nm left ~50% SiO2 masking (GCA Calibration pattern) [1]
1/12/22 DJ_InPRidge 4.5 x 3 13.5 0.563 76.4nm left ~50% SiO2 masking (GCA Calibration pattern) [2]
1/12/22 DJ_InP#3 4.5 x 3 13.5 0.612 71nm left ~50% SiO2 masking (GCA Calibration pattern) [3]
1/26/22 NP_? 10 x 10 100 ~30-40% SiO2 masking (NingC's pattern)
1/26/22 NP_? 1/4 of 50mm wafer 490 0.428-0.46 428nm left ~30-40% SiO2 masking (NingC's pattern) [1]