https://wiki.nanofab.ucsb.edu/w/index.php?title=Old_Deposition_Data_-_2021-12-15&diff=159498&oldid=prev
John d: /* Ion Beam Deposition (Veeco NEXUS) */ added IBD Cals spreadsheet
2021-12-16T07:18:06Z
<p><span dir="auto"><span class="autocomment">Ion Beam Deposition (Veeco NEXUS): </span> added IBD Cals spreadsheet</span></p>
<table class="diff diff-contentalign-left diff-editfont-monospace" data-mw="interface">
<col class="diff-marker" />
<col class="diff-content" />
<col class="diff-marker" />
<col class="diff-content" />
<tr class="diff-title" lang="en">
<td colspan="2" style="background-color: #fff; color: #202122; text-align: center;">← Older revision</td>
<td colspan="2" style="background-color: #fff; color: #202122; text-align: center;">Revision as of 07:18, 16 December 2021</td>
</tr><tr>
<td colspan="2" class="diff-lineno">Line 319:</td>
<td colspan="2" class="diff-lineno">Line 319:</td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>From [[Sputtering Recipes]] page:</div></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>From [[Sputtering Recipes]] page:</div></td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
</tr>
<tr>
<td class="diff-marker">−</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #ffe49c; vertical-align: top; white-space: pre-wrap;"><div>=<del class="diffchange diffchange-inline"> </del>[[Ion Beam Deposition (Veeco NEXUS)]]<del class="diffchange diffchange-inline"> </del>=</div></td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>=[[Ion Beam Deposition (Veeco NEXUS)]]=</div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>*[https://docs.google.com/spreadsheet/ccc?key=0AuBs1GfMrpnXcEdXanZQNko3X0lUcHhVUlNyYnVDUkE&usp=sharing IBD Calibrations Spreadsheet] - Records of historical film depositions (rates, indices), Uniformity etc.</div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>**'''Users may to enter their calibration deps (simple test deps only)'''</div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>* [https://docs.google.com/spreadsheets/d/1y704PRxvXf8bbqb79CrISnk2t0FeojYVJIjrAcBU2_w/edit#gid=sharing Particulates in SiO2 and Ta2O5 in 2015]</div></td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>===SiO{{sub|2}} deposition (IBD)===</div></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>===SiO{{sub|2}} deposition (IBD)===</div></td>
</tr>
</table>
John d
https://wiki.nanofab.ucsb.edu/w/index.php?title=Old_Deposition_Data_-_2021-12-15&diff=159497&oldid=prev
John d: /* Ion Beam Deposition (Veeco NEXUS) */ promoted to Page Title
2021-12-16T07:15:49Z
<p><span dir="auto"><span class="autocomment">Ion Beam Deposition (Veeco NEXUS): </span> promoted to Page Title</span></p>
<table class="diff diff-contentalign-left diff-editfont-monospace" data-mw="interface">
<col class="diff-marker" />
<col class="diff-content" />
<col class="diff-marker" />
<col class="diff-content" />
<tr class="diff-title" lang="en">
<td colspan="2" style="background-color: #fff; color: #202122; text-align: center;">← Older revision</td>
<td colspan="2" style="background-color: #fff; color: #202122; text-align: center;">Revision as of 07:15, 16 December 2021</td>
</tr><tr>
<td colspan="2" class="diff-lineno">Line 319:</td>
<td colspan="2" class="diff-lineno">Line 319:</td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>From [[Sputtering Recipes]] page:</div></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>From [[Sputtering Recipes]] page:</div></td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
</tr>
<tr>
<td class="diff-marker">−</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #ffe49c; vertical-align: top; white-space: pre-wrap;"><div><del class="diffchange diffchange-inline">=</del>= [[Ion Beam Deposition (Veeco NEXUS)]] <del class="diffchange diffchange-inline">=</del>=</div></td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>= [[Ion Beam Deposition (Veeco NEXUS)]] =</div></td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>===SiO{{sub|2}} deposition (IBD)===</div></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>===SiO{{sub|2}} deposition (IBD)===</div></td>
</tr>
</table>
John d
https://wiki.nanofab.ucsb.edu/w/index.php?title=Old_Deposition_Data_-_2021-12-15&diff=159496&oldid=prev
John d: /* SiO2 deposition (IBD) */ added old IBD data
2021-12-16T07:15:12Z
<p><span dir="auto"><span class="autocomment">SiO2 deposition (IBD): </span> added old IBD data</span></p>
<table class="diff diff-contentalign-left diff-editfont-monospace" data-mw="interface">
<col class="diff-marker" />
<col class="diff-content" />
<col class="diff-marker" />
<col class="diff-content" />
<tr class="diff-title" lang="en">
<td colspan="2" style="background-color: #fff; color: #202122; text-align: center;">← Older revision</td>
<td colspan="2" style="background-color: #fff; color: #202122; text-align: center;">Revision as of 07:15, 16 December 2021</td>
</tr><tr>
<td colspan="2" class="diff-lineno">Line 3:</td>
<td colspan="2" class="diff-lineno">Line 3:</td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>From [[PECVD Recipes]] page:</div></td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>{{recipes|Vacuum Deposition}}</div></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>{{recipes|Vacuum Deposition}}</div></td>
</tr>
<tr>
<td colspan="2" class="diff-lineno">Line 312:</td>
<td colspan="2" class="diff-lineno">Line 313:</td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>––––––––––––––––––––––––––––––––––––––––––</div></td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>––––––––––––––––––––––––––––––––––––––––––</div></td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>From [[Sputtering Recipes]] page:</div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>== [[Ion Beam Deposition (Veeco NEXUS)]] ==</div></td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>===SiO{{sub|2}} deposition (IBD)===</div></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>===SiO{{sub|2}} deposition (IBD)===</div></td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
</tr>
<tr>
<td class="diff-marker">−</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #ffe49c; vertical-align: top; white-space: pre-wrap;"><div>====<del class="diffchange diffchange-inline"> </del>SiO<sub>2</sub> Historical Data<del class="diffchange diffchange-inline"> </del>====</div></td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>====SiO<sub>2</sub> Historical Data====</div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"></td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>*[//wiki.nanotech.ucsb.edu/wiki/images/8/8d/New_IBD_SiO2_Standard_Recipe.pdf SiO<sub>2</sub> Standard Recipe]</div></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>*[//wiki.nanotech.ucsb.edu/wiki/images/8/8d/New_IBD_SiO2_Standard_Recipe.pdf SiO<sub>2</sub> Standard Recipe]</div></td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dFRJLUZUdXB4WFA1S1BMMWQ4WndpTWc&usp=drive_web#gid=sharing SiO<sub>2</sub> Data December 2014]</div></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dFRJLUZUdXB4WFA1S1BMMWQ4WndpTWc&usp=drive_web#gid=sharing SiO<sub>2</sub> Data December 2014]</div></td>
</tr>
<tr>
<td colspan="2" class="diff-lineno">Line 363:</td>
<td colspan="2" class="diff-lineno">Line 370:</td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>===Ta{{sub|2}}O{{sub|5}} deposition (IBD)===</div></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>===Ta{{sub|2}}O{{sub|5}} deposition (IBD)===</div></td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
</tr>
<tr>
<td class="diff-marker">−</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #ffe49c; vertical-align: top; white-space: pre-wrap;"><div>====<del class="diffchange diffchange-inline"> </del>Ta2O5 Historical Data (IBD)<del class="diffchange diffchange-inline"> </del>====</div></td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>====Ta2O5 Historical Data (IBD)====</div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"></td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>*[//wiki.nanotech.ucsb.edu/wiki/images/8/85/IBD_Ta2O5_deposition_details.pdf Ta{{sub|2}}O{{sub|5}} Standard Recipe]</div></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>*[//wiki.nanotech.ucsb.edu/wiki/images/8/85/IBD_Ta2O5_deposition_details.pdf Ta{{sub|2}}O{{sub|5}} Standard Recipe]</div></td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dGhhUGdCR2JudkZJU3pBemR4bS1GWWc#gid=0=sharing Ta{{sub|2}}O{{sub|5}} Data December 2014]</div></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dGhhUGdCR2JudkZJU3pBemR4bS1GWWc#gid=0=sharing Ta{{sub|2}}O{{sub|5}} Data December 2014]</div></td>
</tr>
<tr>
<td colspan="2" class="diff-lineno">Line 375:</td>
<td colspan="2" class="diff-lineno">Line 383:</td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>*[https://docs.google.com/spreadsheets/d/1U7XUvluOpgD7tsciZ1pAFGiFsKJKvym6mH5hKaSt5b0/edit#gid=sharing Ta{{sub|2}}O{{sub|5}} Thickness uniformity-1hr depositions 2016]</div></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>*[https://docs.google.com/spreadsheets/d/1U7XUvluOpgD7tsciZ1pAFGiFsKJKvym6mH5hKaSt5b0/edit#gid=sharing Ta{{sub|2}}O{{sub|5}} Thickness uniformity-1hr depositions 2016]</div></td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
</tr>
<tr>
<td class="diff-marker">−</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #ffe49c; vertical-align: top; white-space: pre-wrap;"><div>====<del class="diffchange diffchange-inline"> </del>Ta2O5 Deposition/Film Properies (IBD)<del class="diffchange diffchange-inline"> </del>====</div></td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>====Ta2O5 Deposition/Film Properies (IBD)====</div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"></td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>*Ta2O5 1hr depositions:</div></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>*Ta2O5 1hr depositions:</div></td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>*Deposition Rate: ≈ 7.8 nm/min (users must calibrate this prior to critical deps)</div></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>*Deposition Rate: ≈ 7.8 nm/min (users must calibrate this prior to critical deps)</div></td>
</tr>
</table>
John d
https://wiki.nanofab.ucsb.edu/w/index.php?title=Old_Deposition_Data_-_2021-12-15&diff=159495&oldid=prev
John d: pasted Old (2021-12-15) IBD recipe data
2021-12-16T07:12:09Z
<p>pasted Old (2021-12-15) IBD recipe data</p>
<table class="diff diff-contentalign-left diff-editfont-monospace" data-mw="interface">
<col class="diff-marker" />
<col class="diff-content" />
<col class="diff-marker" />
<col class="diff-content" />
<tr class="diff-title" lang="en">
<td colspan="2" style="background-color: #fff; color: #202122; text-align: center;">← Older revision</td>
<td colspan="2" style="background-color: #fff; color: #202122; text-align: center;">Revision as of 07:12, 16 December 2021</td>
</tr><tr>
<td colspan="2" class="diff-lineno">Line 310:</td>
<td colspan="2" class="diff-lineno">Line 310:</td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>*SiNx etches at 20nm/min</div></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>*SiNx etches at 20nm/min</div></td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>*SiO2 etches at 40nm/min</div></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>*SiO2 etches at 40nm/min</div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>===SiO{{sub|2}} deposition (IBD)===</div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>==== SiO<sub>2</sub> Historical Data ====</div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>*[//wiki.nanotech.ucsb.edu/wiki/images/8/8d/New_IBD_SiO2_Standard_Recipe.pdf SiO<sub>2</sub> Standard Recipe]</div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dFRJLUZUdXB4WFA1S1BMMWQ4WndpTWc&usp=drive_web#gid=sharing SiO<sub>2</sub> Data December 2014]</div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dGNyV083bmpzMjZpZ0JFVWhoOUpaN3c#gid=sharing SiO<sub>2</sub> Thickness uniformity 2014]</div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>*[https://docs.google.com/spreadsheets/d/1pxQkTm274CVjzlnE3cZgE5ycgXfIk8cVCAwTg5x7Xx4/edit#gid=sharing SiO<sub>2</sub> Data-15min depositions 2015]</div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>*[https://docs.google.com/spreadsheets/d/1vYSV7iGIMJsqmlxF6bAjdzuaATcDGxBvwlhb2XYJoWg/edit#gid=sharing SiO<sub>2</sub> Thickness uniformity-15 min depositions 2015]</div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>*[https://docs.google.com/spreadsheets/d/1qnlny3A8jRUPU-8O1ycx9MUFmpti_pRv93rT1pXHMWM/edit#gid=1868267914=sharing SiO<sub>2</sub> Data-1hr depositions 2015]</div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>*[https://docs.google.com/spreadsheets/d/12SKWvqxDuyTgWL44wfvrA2gKDy6ihV2XWh6WJsTT9hE/edit#gid=sharing SiO<sub>2</sub> Thickness uniformity-1hr depositions 2015]</div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>*[https://docs.google.com/spreadsheets/d/1KPLP68f9oC6H2C39r4_Lcd9RkjPiVnZTiz6sMYoJodc/edit#gid=1868267914=sharing SiO<sub>2</sub> Data-1hr depositions 2016]</div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>*[https://docs.google.com/spreadsheets/d/1dFI1B2WxS7oEGMPl2dlLtmiAin-6EKWSEj9hFezB4_w/edit#gid==sharing SiO<sub>2</sub> Thickness uniformity-1hr depositions 2016]</div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>====SiO<sub>2</sub> 1hr deposition properties:====</div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>*Dep.rate: ≈ 5.2 nm/min (users must calibrate this prior to critical deps)</div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>*HF e.r.~350 nm/min</div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>*Stress ≈ -390MPa (compressive)</div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>*Refractive Index: ≈ 1.494</div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>*[[http://en.wikipedia.org/wiki/Cauchy's_equation Cauchy Parameters]] (350-2000nm): </div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>**A = 1.480</div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>**B = 0.00498</div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>**C = -3.2606e-5</div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>===Si<sub>3</sub>N<sub>4</sub> deposition (IBD)===</div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>*[//wiki.nanotech.ucsb.edu/wiki/images/d/d3/IBD_SiNdeposition.pdf Si<sub>3</sub>N<sub>4</sub> Standard Recipe]</div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dDE4RldRQnA1N1ptOUlHQVc3QjNXSkE#gid=sharing Si<sub>3</sub>N<sub>4</sub> Data December 2014]</div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dEdsbWRhYW9mbFRLem56TjFFWjRwR1E#gid=sharing Si<sub>3</sub>N<sub>4</sub> Thickness uniformity 2014]</div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>*Deposition Rate: ≈ 4.10 nm/min (users must calibrate this prior to critical deps)</div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>*HF e.r.~11nm/min</div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>*Stress ≈ -1590MPa (compressive)</div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>*Refractive Index: ≈ 1.969</div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>*[[http://en.wikipedia.org/wiki/Cauchy's_equation Cauchy Parameters]] (350-2000nm): </div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>**A = 2.000</div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>**B = 0.01974</div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>**C = 1.2478e-4</div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>===SiO<sub>x</sub>N<sub>y</sub> deposition (IBD)===</div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>These are some old (2010), initial characterizations only. A recipe improvement would be to increase the Assist O2+N2 = 60sccm total, increasing repeatability. Contact [[Demis D. John|Demis]] for more info.</div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>{|</div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>![[File:IBD SiON Index @ 623nm vs. O2 Gas Flow - v3 - wiki.jpg|alt=plot showing varying refractive index between Si3N4 and SiO2|none|thumb|250x250px|IBD SiO<sub>x</sub>N<sub>y</sub>: Refractive Index vs. O2/N2 Flow.]]</div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>![[File:IBD SiON - Dep rate vs O2 flow - wiki.png|alt=Rate varies monotonically from 53-5 Å/min.|none|thumb|Dep. Rate of IBD SiO<sub>x</sub>N<sub>y</sub> vs. Assist O<sub>2</sub> flow.]]</div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>|}</div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>===Ta{{sub|2}}O{{sub|5}} deposition (IBD)===</div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>==== Ta2O5 Historical Data (IBD) ====</div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>*[//wiki.nanotech.ucsb.edu/wiki/images/8/85/IBD_Ta2O5_deposition_details.pdf Ta{{sub|2}}O{{sub|5}} Standard Recipe]</div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dGhhUGdCR2JudkZJU3pBemR4bS1GWWc#gid=0=sharing Ta{{sub|2}}O{{sub|5}} Data December 2014]</div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dE5xbVFyUFZqdTdUN0JRSUNvMGFGb2c#gid=sharing Ta{{sub|2}}O{{sub|5}} Thickness uniformity 2014]</div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>*[https://docs.google.com/spreadsheets/d/1WRqzTTIX4D7Un-XqHqSB66JuSplrMiZAzGvjYFZ-Gtk/edit#gid=sharing Ta{{sub|2}}O{{sub|5}} Data December-15 min depositions 2015]</div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>*[https://docs.google.com/spreadsheets/d/1BZrNtzHwWqfLhvZW4UY01CUfkObW70MxW9jdLhBcunc/edit#gid=sharing Ta{{sub|2}}O{{sub|5}} Thickness uniformity-15 min depositions 2015]</div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>*[https://docs.google.com/spreadsheets/d/1saOA_9SwcPCkuW7uGgOSXhvtwrMkKJUxeS4wRE9qxQ8/edit#gid=sharing Ta{{sub|2}}O{{sub|5}} Data December-1hr depositions 2015]</div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>*[https://docs.google.com/spreadsheets/d/1wXAtWbbE8dvvulJxJXkwQyejgcrz51t-HH4omTq0scs/edit#gid=sharing Ta{{sub|2}}O{{sub|5}} Thickness uniformity-1hr depositions 2015]</div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>*[https://docs.google.com/spreadsheets/d/1A0bVnVgwPfj5JfAtmgNSeto2Rix8qOfiGO9mpXa433g/edit#gid=sharing Ta{{sub|2}}O{{sub|5}} Data December-1hr depositions 2016]</div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>*[https://docs.google.com/spreadsheets/d/1U7XUvluOpgD7tsciZ1pAFGiFsKJKvym6mH5hKaSt5b0/edit#gid=sharing Ta{{sub|2}}O{{sub|5}} Thickness uniformity-1hr depositions 2016]</div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>==== Ta2O5 Deposition/Film Properies (IBD) ====</div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>*Ta2O5 1hr depositions:</div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>*Deposition Rate: ≈ 7.8 nm/min (users must calibrate this prior to critical deps)</div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>*HF e.r.~2 nm/min</div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>*Stress ≈ -232MPa (compressive)</div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>*Refractive Index: ≈ 2.172</div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>*[[http://en.wikipedia.org/wiki/Cauchy's_equation Cauchy Parameters]] (350-2000nm): </div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>**A = 2.1123</div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>**B = 0.018901</div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>**C = -0.016222</div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>===TiO{{sub|2}} deposition (IBD)===</div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>*[//wiki.nanotech.ucsb.edu/wiki/images/3/3b/New_IBD_TiO2_deposition.pdf TiO<sub>2</sub> Standard Recipe]</div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dGVXVkM4dEdXaU15M09HNGhJbGUycVE#gid=sharing TiO<sub>2</sub> Data December 2014]</div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dF9YSW9jTDJzY19MbmVEbUQtVzJVdVE#gid=sharing TiO<sub>2</sub> Thickness uniformity 2014]</div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>*Deposition Rate: ≈ 1.29 nm/min (users must calibrate this prior to critical deps)</div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>*HF etch rate ~5.34nm/min</div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>*Stress ≈ -445MPa (compressive)</div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>*Refractive Index: ≈ 2.259</div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>*[[http://en.wikipedia.org/wiki/Cauchy's_equation Cauchy Parameters]] (350-2000nm): </div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>**A = 2.435</div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>**B = -4.9045e-4</div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>**C = 0.01309</div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>*Absorbing < ~350nm</div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>===Al<sub>2</sub>O<sub>3</sub> deposition (IBD)===</div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>*Al2O3 standard recipe: 1_Al2O3_dep</div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>*[https://docs.google.com/spreadsheets/d/1Qwxa7rtq2kGeFUQxnjGFgtdCJP4uIX_bdUcCWFvO72g/edit#gid= Al2O3 Data 2018]</div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>*[https://docs.google.com/spreadsheets/d/1rjwDQ0WJOIL7XWx2KWQ4fEPjNkr6GEmiXGmQXZnWFOI/edit#gid= Al2O3 Thickness uniformity 2018]</div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>*Deposition Rate: ≈ 2.05nm/min (users must calibrate this prior to critical deps)</div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>*HF etch rate ~167nm/min</div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>*Stress ≈ -332MPa (compressive)</div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>*Refractive Index: ≈ 1.656</div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>*[[http://en.wikipedia.org/wiki/Cauchy's_equation Cauchy Parameters]] (350-2000nm):( working on) </div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>**A =</div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>**B =</div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>**C =</div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>*Absorbing < ~350nm</div></td>
</tr>
</table>
John d
https://wiki.nanofab.ucsb.edu/w/index.php?title=Old_Deposition_Data_-_2021-12-15&diff=159488&oldid=prev
John d: Created page with "OLD Data: Copied on 2021-12-14 {{recipes|Vacuum Deposition}} =PECVD 1 (PlasmaTherm 790)= ====Historical Particulate Data==== *[https://docs.google.com/spreadsheets/d..."
2021-12-15T14:35:56Z
<p>Created page with "OLD Data: Copied on 2021-12-14 {{recipes|Vacuum Deposition}} =<a href="/wiki/PECVD_1_(PlasmaTherm_790)" title="PECVD 1 (PlasmaTherm 790)">PECVD 1 (PlasmaTherm 790)</a>= ====Historical Particulate Data==== *[https://docs.google.com/spreadsheets/d..."</p>
<p><b>New page</b></p><div>OLD Data: <br />
Copied on 2021-12-14<br />
<br />
<br />
<br />
{{recipes|Vacuum Deposition}}<br />
<br />
=[[PECVD 1 (PlasmaTherm 790)]]=<br />
====Historical Particulate Data====<br />
<br />
*[https://docs.google.com/spreadsheets/d/1a0XrY6HuJ6L9niThZYI-u4XH69Hnbe3jkm1qKmrR8Rg/edit#gid=sharing Particulates(Gain4) in PECVD#1-OLD DATA 2015]<br />
*[https://docs.google.com/spreadsheets/d/1ZfkspbCQZmdThC8qB4XyjsyPAzrMF1QbHSMFmH6xSo4/edit#gid=sharing Particulates(Gain4) in PECVD#1-OLD DATA 2016]<br />
*[https://docs.google.com/spreadsheets/d/1YNiof68Veeh08s_NtG5aCWUXW7GWDDU00HAimV_l8_g/edit#gid=sharing Particulates(Gain4) in PECVD#1-OLD DATA 2017]<br />
*[https://docs.google.com/spreadsheets/d/1VN551M2oXGWX306HDLQXvZIp3kgxEvWffQqMqnc8ISk/edit#gid=sharing Particulates in PECVD#1 films 2017]<br />
*[https://docs.google.com/spreadsheets/d/11c0gQHnattIjVO95aBqiL-zL4DInRFihV-YB54xLT40/edit#gid=sharing Particulates in PECVD#1 films 2018]<br />
*[https://docs.google.com/spreadsheets/d/1ct-SSCRxf81W0jupCWzh81n0DBwPv6mwKFMzuWu_0TI/edit#gid=sharing Particulates in PECVD#1 films 2019]<br />
*[https://docs.google.com/spreadsheets/d/1yks0OgH8rpbYjin_Qr8vpPg8jBiZQRs_PKfyfo-Rqg0/edit#gid=sharing Particulates in PECVD#1 films 2020]<br />
*[https://docs.google.com/spreadsheets/d/1vSmymaS_NNXW-ouC8Ky1J6iVSla7uyRB2zf1lGMa31g/edit#gid=sharing Particulates in PECVD#1 films 2021]<br />
<br />
==SiN deposition (PECVD #1)==<br />
<br />
*[https://docs.google.com/spreadsheets/d/1DGU745SeunYz4sLs1LpGKbtOYX-tQyBHEvVYcMxHRKE/edit#gid= Si3N4 Standard Recipe]<br />
<br />
====Historical Data====<br />
=====Thin-Film Properties=====<br />
<br />
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dEN6LV93LXlnbUhIWU1adVZWMWlXYnc&usp=drive_web#gid=sharing SiN 100nm Data 2014]<br />
*[https://docs.google.com/spreadsheets/d/1phx1WficlUEg0xSahaAq4zrRk6m9Eb0ausO8wcAmXqs/edit#gid=sharing SiN 100nm Data 2015]<br />
*[https://docs.google.com/spreadsheets/d/1VNSNTqnbE4SFk0HyhBAy3GJzi0jRQEs8cgk1v2_Uam8/edit#gid=sharing SiN 100nm Data 2016]<br />
*[https://docs.google.com/spreadsheets/d/1TG1X2wpl2fWaHEtAHtpZFBVSCk1BQeGJQ8LA2M2qBJ0/edit#gid=sharing SiN 100nm Data 2017]<br />
*[https://docs.google.com/spreadsheets/d/1UlyvPcXUBQ5R2JwjKOjELvtCJaTElVhJHfzgjyaRd2A/edit#gid=sharing SiN 300nm Data 2017]<br />
*[https://docs.google.com/spreadsheets/d/1pAoTCaNSf0uZMyiQ2qKFd0s_e4e53P9Z1jUwtmTnlLk/edit#gid=sharing SiN 300nm Data 2018]<br />
*[https://docs.google.com/spreadsheets/d/1Pnw8eEaQ0rGblRYl6LeIm6wrh1hgeyjnHEbA4BzV8JM/edit#gid=sharing SiN 300nm Data 2019]<br />
*[https://docs.google.com/spreadsheets/d/1N_1Kk6J-wA4nlHpFg5EMDZNHR1kLDo_fr_Dvc6osSr4/edit#gid=sharing SiN 300nm Data 2020]<br />
*[https://docs.google.com/spreadsheets/d/13jY5T_PW1a3GjHIbR0GuUbIhmxClQfvLgzaUtl3YniE/edit#gid=sharing SiN 300nm Data 2021]<br />
<br />
=====Uniformity Data=====<br />
<br />
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dElmTXZyOEZsOFdrMVhNLWpKXzVmNWc&usp=sharing SiN 100 nm Thickness uniformity 2014]<br />
*[https://docs.google.com/spreadsheets/d/1-pET1Eojooso5UHk90W-5uYByDDdrCyRnggqewxTmVg/edit#gid=sharing SiN 100 nm Thickness uniformity 2015]<br />
*[https://docs.google.com/spreadsheets/d/1V_-KzsdR-2tSnJGtUdQWokmnNIY949t0vdQOp7RfCgc/edit#gid=sharing SiN 100 nm Thickness uniformity 2016]<br />
*[https://docs.google.com/spreadsheets/d/1tM-a4VBEqpxr2G8PGGLTbsR6BQBmvqXNRBw0mikAUS0/edit#gid=sharing SiN 100 nm Thickness uniformity 2017]<br />
*[https://docs.google.com/spreadsheets/d/1Z83RCH5cAUfViO6vv6hAatcLVWZ95ex4nDdfffm9I7s/edit#gid=sharing SiN 300nm Thickness uniformity 2017]<br />
*[https://docs.google.com/spreadsheets/d/1b4EQZdRtVbqNwGBrItoG5-tz6RIzlsvBiCFR6ZXfylw/edit#gid=sharing SiN 300nm Thickness uniformity 2018]<br />
*[https://docs.google.com/spreadsheets/d/1-OiaH8frAzJzHKfbYTJP808ddzk1Wsv_CixDzG-sSfo/edit#gid=sharing SiN 300nm Thickness uniformity 2019]<br />
*[https://docs.google.com/spreadsheets/d/1e5ycwODa-VooEzGjhY4XquvJpuAuIQHHHZSRwZaH5-E/edit#gid=sharing SiN 300nm Thickness uniformity 2020]<br />
*[https://docs.google.com/spreadsheets/d/1Re5xwB5WMgsgDHsi_0dUeL62uWAnqDQtoBoaR7lj8cI/edit#gid=sharing SiN 300nm Thickness uniformity 2021]<br />
<br />
==SiO<sub>2</sub> deposition (PECVD #1)==<br />
<br />
*[https://docs.google.com/spreadsheets/d/1uqpg3sirsRbXdTFlxZ6_k3t0ovP0MtpFtICjpH0-prs/edit#gid= SiO2 Standard Recipe]<br />
<br />
====Historical Data====<br />
=====Thin-Film Properties=====<br />
<br />
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dEw0bjFEdTF2SUhRa25Ca0d0SzBha3c&usp=drive_web#gid=sharing SiO<sub>2</sub> 100nm Data 2014]<br />
*[https://docs.google.com/spreadsheets/d/1JWNUcH8l90xif-0BhYKJee9nXxE4hnvvp6N2NtZLYXY/edit#gid=sharing SiO<sub>2</sub> 100nm Data 2015]<br />
*[https://docs.google.com/spreadsheets/d/1F2pfsVnbUgaE9tsm8HZMlY6cyt-nhui0IpvGc6udhDU/edit#gid=sharing SiO<sub>2</sub> 100nm Data 2016]<br />
*[https://docs.google.com/spreadsheets/d/1MblK5Zr5Skfw0s9Hdhqr_cCwN-nCgM-ofZnsAyvVRq8/edit#gid=sharing SiO<sub>2</sub> 100nm Data 2017]<br />
*[https://docs.google.com/spreadsheets/d/15SocIqWQvBKSvT5oCWoZAURLaaqb9KosxCN2rueZQN8/edit#gid=sharing SiO<sub>2</sub> 300nm Data 2017]<br />
*[https://docs.google.com/spreadsheets/d/1DdjIRGsfJ7WCrxQoGpmzkjLGJhpBTFNYLFmmHcNjAjk/edit#gid=sharing SiO<sub>2</sub> 300nm Data 2018]<br />
*[https://docs.google.com/spreadsheets/d/1QbhukSuVNueT067IVEpweSlD4B7GQecf-tfQFQeV6Xs/edit#gid=sharing SiO<sub>2</sub> 300nm Data 2019]<br />
*[https://docs.google.com/spreadsheets/d/1OwyhfFPDH-XLPczA8cKoBPnujq9oNukaWkHq0KoFS40/edit#gid=sharing SiO<sub>2</sub> 300nm Data 2020]<br />
*[https://docs.google.com/spreadsheets/d/1I-0Ih_F9pWeOwXeEQC6IFYKNB6bBLSoBiyX8Eu3pwFg/edit#gid=sharing SiO<sub>2</sub> 300nm Data 2021]<br />
<br />
=====Thick-Film Properties=====<br />
<br />
*[https://docs.google.com/spreadsheets/d/1XgUlCaCv3jCK9RyrI553PkIS0PmiAlbWjsDwK5TOH3I/edit#gid=sharing SiO<sub>2</sub> Thick film Data 2021]<br />
<br />
====Uniformity Data====<br />
<br />
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dDQ3VEtZQVRpdVdlbGtIZHpTNmFzNmc&usp=drive_web#gid=sharing SiO<sub>2</sub> 100nm Thickness uniformity 2014]<br />
*[https://docs.google.com/spreadsheets/d/1NQy-ADou6f2NBU-9jZG8KME1lOz0X5mh6HZV9_jPGes/edit#gid=sharing SiO<sub>2</sub> 100 nm Thickness uniformity 2015]<br />
*[https://docs.google.com/spreadsheets/d/1WUCm_dWpxKTjfFf1rNfLuxvwMxsyCYON_OZ3gb50L_s/edit#gid=sharing SiO<sub>2</sub> 100 nmThickness uniformity 2016]<br />
*[https://docs.google.com/spreadsheets/d/1dpC_AkPD-etIH6fVuQqLfd4UMNQCEtcqhvmBpwbEncE/edit#gid=sharing SiO<sub>2</sub> 100nm Thickness uniformity 2017]<br />
*[https://docs.google.com/spreadsheets/d/1Fa8mZIBIeJwvCwUbJ-28VcvVYj8rshhuDuXsYxA-cD8/edit#gid=sharing SiO<sub>2</sub> 300nm Thickness uniformity 2017]<br />
*[https://docs.google.com/spreadsheets/d/1YB_9USpuXGpIdSW2gNsptu5nSrLWAGsYu0SWoYEy0aQ/edit#gid=sharing SiO<sub>2</sub> 300nm Thickness uniformity 2018]<br />
*[https://docs.google.com/spreadsheets/d/1FatUAEegWuDRzVa47L1_cqgRs0AZ_Fao9jpwz5sfln0/edit#gid=sharing SiO<sub>2</sub> 300nm Thickness uniformity 2019]<br />
*[https://docs.google.com/spreadsheets/d/1uAIEv_z2TJtY2XxTYnDIyKwKT4ZIhalTCyZ5SrDRJmA/edit#gid=sharing SiO<sub>2</sub> 300nm Thickness uniformity 2020]<br />
*[https://docs.google.com/spreadsheets/d/1jThamYtEiH3lVz4IzoG9ILxBG8-TufIKnUd8V0qKQU0/edit#gid=sharing SiO<sub>2</sub> 300nm Thickness uniformity 2021]<br />
<br />
==Low-Stress SiN - LS-SiN (PECVD#1)==<br />
<br />
*[https://wiki.nanotech.ucsb.edu/wiki/images/4/4a/New_PECVD1-LS_SIN-Turner05recipe_2014_LS_SIN_recipe.pdf LS SiN Standard Recipe]<br />
*[https://docs.google.com/spreadsheets/d/1Joz0az9TGZWQc4CiMQJZzLBbNFbx_hH2Oc0B4NNJmYk/edit#gid=sharing LS SiN Data 2014]<br />
*[https://docs.google.com/spreadsheets/d/1xIzc2CufRYNSfAtsOXpw3IzHreeu42BWrLBV0kzP6kA/edit#gid=sharing LS SiN 1000A Thickness uniformity 2014]<br />
<br />
==SiO<sub>x</sub>N<sub>y</sub> deposition (PECVD #1)==<br />
<br />
*[https://wiki.nanotech.ucsb.edu/wiki/images/2/24/New_PECVD1-LS_SION-recipe_2014_LS_SION_recipe.pdf SiO<sub>x</sub>N<sub>y</sub> Standard Recipe]<br />
*[https://docs.google.com/spreadsheets/d/1rixyzAAq6q08M5OwvZiDVoh3K8B566XKM-UZAQIAnsg/edit#gid=sharing SiO<sub>x</sub>N<sub>y</sub> Data 2014]<br />
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dEttR2JSTkRoamR0SUZ4bE5QUW9uS2c&usp=sharing SiO<sub>x</sub>N<sub>y</sub>1000A Thickness uniformity 2014]<br />
<br />
==Cleaning Recipes (PECVD #1)==<br />
The cleaning procedure is very important in order to have consistent result on this tool and also to keep particulate count low. After each deposition you should clean the tool following instructions carefully. The clean is done in two steps: <br />
<br />
#Wet cleaning (start cleaning by using a cleanroom wipe sprayed with DI. Wipe chamber sidewalls with it. Finish cleaning by using the cleanroom wipe sprayed with IPA. )<br />
#Load the recipe for cleaning "CF4/O2 Clean" (edit the recipe and change ONLY time of cleaning). Follow instructions regarding a required time for cleaning.<br />
<br />
===[https://wiki.nanotech.ucsb.edu/w/images/7/72/PECVD1-cleaning.png Standard Cleaning Recipe: "CF4/O2 Clean"]===<br />
Click the above link for a screenshot of the standard cleaning recipe, for which you will enter a custom time. The recipe is set up so that it will '''pop up a window for the cleaning time upon running the recipe''' - you do not need to edit the recipe before running it.<br />
=[[PECVD 2 (Advanced Vacuum)]]=<br />
====Historical Particulate Data====<br />
<br />
*[https://docs.google.com/spreadsheets/d/1kj0SWxRpnPRoGld8k3sW-3yK1iPm3buTkvlJSN5YPV4/edit#gid=sharing Particulates (Gain4) in PECVD#2 2015]<br />
*[https://docs.google.com/spreadsheets/d/1xpk9tJrE68NIJ_1yIym0xBxd4fnzHHBHdkhFehruO3E/edit#gid=sharing Particulates (Gain4) in PECVD#2 2016]<br />
*[https://docs.google.com/spreadsheets/d/1ICgt-fgTvNPbE_65x5jUsqy8JjHVv5WUvmE7g7VUbsI/edit#gid=sharing Particulates (Gain4) in PECVD#2 2017]<br />
<br />
*[https://docs.google.com/spreadsheets/d/1yPAPP24z3RcRRi-HqEp3GJN4JM8Ec8SFJwZ-OYGG2HU/edit#gid=sharing Particulates in PECVD#2 films 2017]<br />
*[https://docs.google.com/spreadsheets/d/1aU6fTyQ5MlGD4uCa9gepG5rLJzW3wlkOWSKEl_w_Ye4/edit#gid=sharing Particulates in PECVD#2 films 2018]<br />
*[https://docs.google.com/spreadsheets/d/1OPZXe8g3H0wywIrPFel3nSZ5iyPs2mVIYUSVKfTtMDg/edit#gid=sharing Particulates in PECVD#2 films 2019]<br />
*[https://docs.google.com/spreadsheets/d/1Y9lomsf7bDojeXoAsEG7xvypx_sw_atpmPwB9xtK1Zk/edit#gid=sharing Particulates in PECVD#2 films 2020]<br />
*[https://docs.google.com/spreadsheets/d/1BauS7q_sGKkaeY6o3BOw2wyQsyS_DukJxCAbGantDW4/edit#gid=sharing Particulates in PECVD#2 films 2021]<br />
<br />
==SiO<sub>2</sub> deposition (PECVD #2)==<br />
====Standard Recipe====<br />
<br /><br />
<br />
*[https://docs.google.com/spreadsheets/d/1wCEcFj6ZMHR4QifngLXwz6dqbyf8hsVKu7bQbMS6EoA/edit#gid= STD SiO2 Recipe]<br />
<br />
====Historical Data====<br />
=====Thin-Film Properties=====<br />
<br />
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dGJZaGtDTVRqa1BRdW5iU1N1Y01jd0E&usp=drive_web#gid=sharing Oxide Data 2014]<br />
*[https://docs.google.com/spreadsheets/d/1d5boeJRWWgMqvQe6nVM7m8s3KAcS4Yp2L5CEU9svkX4/edit#gid=sharing Oxide Data 2015]<br />
*[https://docs.google.com/spreadsheets/d/1XQRcTJdw9AIMPAUsH0n9Ic9Fe1_xGDSvAxD4gVc9FBw/edit#gid=sharing Oxide data 2016]<br />
*[https://docs.google.com/spreadsheets/d/1vcaHwraMGNHuRxgWwGp78EJf4T3Jk182wxoCz_neuck/edit#gid=sharing Oxide Data 2017]<br />
*[https://docs.google.com/spreadsheets/d/1VI-sUmaqois0NsCvf2kQmPfRRa03MjBzl779hmmLtP4/edit#gid=sharing Oxide Data 2018]<br />
*[https://docs.google.com/spreadsheets/d/1oWnQ3D6oknKWU2bohvSrN85rlEZgQN3YP_ZJ4i8u7do/edit#gid=sharing Oxide Data 2019]<br />
*[https://docs.google.com/spreadsheets/d/1Z9UMgaQC2PiLLrMk04mpKWkJLa1L_WFMAm5079eKxI0/edit#gid=sharing Oxide Data 2020]<br />
*[https://docs.google.com/spreadsheets/d/10XA3WnHjUZOLFunwUIlM2IqaRIiX_EGb6Jj_bw84gkI/edit#gid=sharing Oxide Data 2021]<br />
<br />
=====Thin-Film Properties=====<br />
<br />
*[https://docs.google.com/spreadsheets/d/19Z8IAVgumWuH0t8RN23LJ2wWZP7jYYLwRl9pDQP4obI/edit#gid=sharing Thick Oxide Data 2021]<br />
<br />
=====Uniformity Data=====<br />
<br />
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dDRjSHEtYUZRUTg4azE2U0JGUTg2M1E#gid=sharing Oxide Thickness Uniformity 2014]<br />
*[https://docs.google.com/spreadsheets/d/16pZHcGwesXB1mMPwntOudBIlPvRh6A6DI37DEwyYfPw/edit#gid=sharing Oxide Thickness Uniformity 2015]<br />
*[https://docs.google.com/spreadsheets/d/10OEuANVNmHqWvx-92zibechIrHK5kgqSK4B_O_O3-YI/edit#gid=sharing Oxide Thickness Uniformity 2016]<br />
*[https://docs.google.com/spreadsheets/d/19JjJYdFNFzO685Hp9hODVRFAYF5bP3IEYGTRGQjqLN4/edit#gid=sharing Oxide Thickness Uniformity 2017]<br />
*[https://docs.google.com/spreadsheets/d/1064j6894X63WlRX3Uolxg1q1FRzUZLqSZQA9BWwzPOk/edit#gid=sharing Oxide Thickness Uniformity 2018]<br />
*[https://docs.google.com/spreadsheets/d/1064j6894X63WlRX3Uolxg1q1FRzUZLqSZQA9BWwzPOk/edit#gid=sharing Oxide Thickness Uniformity 2019]<br />
*[https://docs.google.com/spreadsheets/d/1Z9UMgaQC2PiLLrMk04mpKWkJLa1L_WFMAm5079eKxI0/edit#gid=sharing Oxide Thickness Uniformity 2020]<br />
*[https://docs.google.com/spreadsheets/d/1b9Fmzp_d-XiMerFtrDiCsmS7NMNoaBtS8T0DLqoii8Y/edit#gid=sharing Oxide Thickness Uniformity 2021]<br />
<br />
==SiN deposition (PECVD #2)==<br />
====Standard Recipe====<br />
<br />
*[https://wiki.nanotech.ucsb.edu/wiki/images/4/4c/SiNx_Films_by_PECVD2.pdf SiNx Film Stress vs LF and HF Duration Time, and Gas Flowing-rate]<br />
*[https://docs.google.com/spreadsheets/d/1KS4HfhUJyYVep4H6CRAKpMRP5TA31F0qD-obQkKRnEI/edit#gid= STD Nitride2 Recipe]<br />
<br />
====Historical Data====<br />
=====Thin-Film Properties=====<br />
<br />
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dDE0R3FlenNPa2txNmRldTczMXZNNnc#gid=sharing Nitride2 Data 2014]<br />
*[https://docs.google.com/spreadsheets/d/1SkYqOwgjUyMaFBPhuTjMvBTXu0KdQFNmITryF_OVi8o/edit#gid=sharing Nitride2 Data 2015]<br />
*[https://docs.google.com/spreadsheets/d/1HJszgZyEZR9ZsiJpQM6pdsoQ6pWwI6brXasdmfDRoBQ/edit#gid=sharing Nitride2 Data 2016]<br />
*[https://docs.google.com/spreadsheets/d/1f3JBEnr7lf0yIMlzlOYKv_bXlIDyXt8vec_rSVJIoOk/edit#gid=sharing Nitride2 Data 2017]<br />
*[https://docs.google.com/spreadsheets/d/1OO0ewGSqYSzL3lj8fXkgckTkBGQRliD6sBc02IW7wZY/edit#gid=sharing Nitride2 Data 2018]<br />
*[https://docs.google.com/spreadsheets/d/1Zi8CRspd3LTDdNRRCneE0--bVohWvZbV_kSHo04s0oI/edit#gid=sharing Nitride2 Data 2019]<br />
*[https://docs.google.com/spreadsheets/d/1LEutQynQXU_9B4EqRt21PX9TGR13IqaMge7sKAXKAfg/edit#gid=sharing Nitride2 Data 2020]<br />
*[https://docs.google.com/spreadsheets/d/1piGMPEHXiUV5WMNfaTFKdL1pnE8W2yrWHkNWHd7Au1A/edit#gid=sharing Nitride2 Data 2021]<br />
<br />
=====Uniformity Data=====<br />
<br />
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dERkYm85bGtYQVpjVk5GTGJuMkg2anc&usp=drive_web#gid=sharing Nitride2 Thickness Uniformity 2014]<br />
*[https://docs.google.com/spreadsheets/d/14_dYQu3z31fF_oxsUUX8BmDucgv6B07xB3_zqP0HmvM/edit#gid=sharing Nitride2 Thickness Uniformity 2015]<br />
*[https://docs.google.com/spreadsheets/d/1qBHs7uALM2OdE-yXOq4uZk6aUQEjZRjG1C6RcMEf0sk/edit#gid=sharing Nitride2 Thickness Uniformity 2016]<br />
*[https://docs.google.com/spreadsheets/d/1WJcYzHUjLrWpys_i-Q96FN_lBDBufpXZKZVEX_gri_Q/edit#gid=sharing Nitride2 Thickness Uniformity 2017]<br />
*[https://docs.google.com/spreadsheets/d/1hzj4Fb5fN8lS0m9-rm9AgEn0Zunif5grI4X7YkAMEFU/edit#gid=sharing Nitride2 Thickness Uniformity 2018]<br />
*[https://docs.google.com/spreadsheets/d/1hzj4Fb5fN8lS0m9-rm9AgEn0Zunif5grI4X7YkAMEFU/edit#gid=sharing Nitride2 Thickness Uniformity 2019]<br />
*[https://docs.google.com/spreadsheets/d/1xdzjLODpe2Xb7r4PGil1q-OFqSYKuZBivqLt1T6lezw/edit#gid=sharing Nitride2 Thickness Uniformity 2020]<br />
*[https://docs.google.com/spreadsheets/d/19x70-CIyQ41pywpL-IusldLv7XYJps9aJT5-rYYQSCs/edit#gid=sharing Nitride2 Thickness Uniformity 2021]<br />
<br />
==Low-Stress SiN deposition (PECVD #2)==<br />
''Low-Stress SilIcon Nitride (< 100 MPa)''<br />
====Standard Recipe====<br />
<br />
*[https://docs.google.com/spreadsheets/d/1DzzI7aE61R7c6gyk6cGBdm9FtGrApiNJ4AL90ll2C8k/edit#gid= STD LS Nitride2 Recipe]<br />
*''Old Versions:''<br />
**[https://wiki.nanotech.ucsb.edu/wiki/images/a/a5/New_AdvPECVD-LS_Nitride2_300C_standard_recipe_LS_Nitride2_standard_recipe.pdf LS Nitride2 Standard Recipe 2014-5/9/2018]<br />
**[https://wiki.nanotech.ucsb.edu/wiki/images/0/01/STD_LSNitride2_5-9-18.pdf STD LSNitride2 5/9/2018]<br />
<br />
====Historical Data====<br />
=====Thin-Film Properties=====<br />
<br />
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dEZvWVhzS1pHUXZkOGcyQWZ4LTNBWGc&usp=drive_web#gid=sharing LS Nitride2 Data 2014]<br />
*[https://docs.google.com/spreadsheets/d/16Q6BrPoNiFP0elVoSGwXRfQdHXzAXOgiyqKmEw-4kII/edit#gid=sharing LS Nitride2 Data 2015]<br />
*[https://docs.google.com/spreadsheets/d/1GZ58eFzD-T8DJ2Nsaj74u6cvawzsOI2DmMit6Z7vqys/edit#gid=sharing LS Nitride2 Data 2016]<br />
*[https://docs.google.com/spreadsheets/d/1gGIWqkCnykPgBc3prhXExT7QcNjWm2HdbTtwugNqm18/edit#gid=sharing LS Nitride2 Data 2017]<br />
*[https://docs.google.com/spreadsheets/d/1vwpDtiglR2DLWiYNhpBX77cyyj9lw55iVeFz1puN7bM/edit#gid=sharing LS Nitride2 Data 2018]<br />
*[https://docs.google.com/spreadsheets/d/1zvSl2P5T926Ol48yH3FBCZm1zCeycl3S8GWQYtzi8VI/edit#gid=sharing LS Nitride2 Data 2019]<br />
*[https://docs.google.com/spreadsheets/d/1muyFsIspqZXB2HXiqG3t39uzeO7A7Srvh4aGdXjwCc4/edit#gid=sharing LS Nitride2 Data 2020]<br />
*[https://docs.google.com/spreadsheets/d/1qzVA44esh71655lE1rrpGkKKNTyZRC_mv3IaiZ_HAWQ/edit#gid=sharing LS Nitride2 Data 2021]<br />
<br />
=====Uniformity Data=====<br />
<br />
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dENSak1ZNnVaVTFEQTBzdDJMSDlDTFE&usp=drive_web#gid=1=sharing LS Nitride2 Thickness Uniformity 2014]<br />
*[https://docs.google.com/spreadsheets/d/1LpkaOpr7oNoyvxFkineD7i9FspO6LweJMulvZHJM5Zc/edit#gid=sharing LS Nitride2 Thickness Uniformity 2015]<br />
*[https://docs.google.com/spreadsheets/d/1FRzW9BaIPF2D3cxPgjLq8hbvrBHXDNkiW6DiPVKQBRM/edit#gid=sharing LS Nitride2 Thickness Uniformity 2016]<br />
*[https://docs.google.com/spreadsheets/d/1vyrgvdEZFgnQUilpa5Ka2nOfowY8zlmJfbQ77EamNBg/edit#gid=sharing LS Nitride2 Thickness Uniformity 2017]<br />
*[https://docs.google.com/spreadsheets/d/17OGrhbvP8O_0mBMIsmUmEwfyFaoJnNNpMFpgBUW7qzI/edit#gid=sharing LS Nitride2 Thickness Uniformity 2018]<br />
*[https://docs.google.com/spreadsheets/d/17OGrhbvP8O_0mBMIsmUmEwfyFaoJnNNpMFpgBUW7qzI/edit#gid=sharing LS Nitride2 Thickness Uniformity 2019]<br />
*[https://docs.google.com/spreadsheets/d/1M4ug8SAqy2Ky70LNLW3pL2MjSs69beJVhbC2BbabHaU/edit#gid=sharing LS Nitride2 Thickness Uniformity 2020]<br />
*[https://docs.google.com/spreadsheets/d/12wvXFHN7CV_XSFj6hB5Gd7SIXERwzkTM__58ZqzPOuk/edit#gid=sharing LS Nitride2 Thickness Uniformity 2021]<br />
<br />
==Amorphous-Si deposition (PECVD #2)==<br />
<br />
*[https://wiki.nanotech.ucsb.edu/wiki/images/9/9d/03-Amorphous-Si-PECVD-2.pdf Amorphous Si Deposition Recipe]<br />
*[https://wiki.nanotech.ucsb.edu/wiki/images/0/09/ASi_deposition_and_film_stress_using_AV_dep_tool.pdf Amorphous Si Films and Their Stress]<br />
<br />
==Cleaning Recipes (PECVD #2)==<br />
===Cleaning Procedure (PECVD#2)===<br />
The cleaning procedure is very important in order to have consistent result on this tool and also to keep particulate count low. After each deposition you should clean the tool following instructions carefully. The clean is done in two steps:<br />
<br />
#(If >29min dep time) Wet cleaning: Start cleaning by using a cleanroom wipe sprayed with DI. Wipe upper chamber sidewalls with it. Finish cleaning by using the cleanroom wipe sprayed with IPA & wiping again.<br />
#Load the recipe for cleaning "STD CF4/O2 Clean" (edit the recipe and change ONLY time of cleaning). Follow instructions regarding required time for cleaning.<br />
<br />
===[https://wiki.nanotech.ucsb.edu/w/images/3/34/PECVD2_photo_for_cleaning.png Standard Clean Recipe: "STD CF4/O2 Clean recipe"]===<br />
Click the above link for a screenshot of the standard cleaning recipe, for which you will enter a custom time. The recipe is set up so that it will '''pop up a window for the cleaning time upon running the recipe''' - you do not need to edit the recipe before running it.<br />
===Clean Times (PECVD#2)===<br />
{| class="wikitable"<br />
!Film Deposited<br />
!Cleaning Time (Dry)<br />
|-<br />
|SiO<sub>2</sub><br />
|1 min. clean for every 1 min. deposition<br />
|-<br />
|Si<sub>3</sub>N<sub>4</sub><br />
|1 min. clean for every 7 min of deposition<br />
|-<br />
|If > 29min total dep time<br />
(Season + Dep)<br />
|Wet Clean the Upper Lid/Chamber<br />
DI water then Isopropyl Alcohol on chamber wall & portholes<br />
|}<br /><br />
=[[ICP-PECVD (Unaxis VLR)]]=<br />
2020-02: New recipes have been characterized for low particulate count and repeatability. Only staff-supplied recipes are allowed in the tool. Please follow the [[ICP-PECVD (Unaxis VLR)#Documentation|'''new procedures''']] to ensure low particle counts in the chamber.<br />
<br />
The system currently has '''Deuterated Silane (SiD<sub>4</sub>) installed''' - identical to the regular Silicon precursor SiH<sub>4</sub>, except that it significantly lowers optical absorption in the near-infrared due to shifted molecular vibrations/molecular weights.<br />
====Historical Particulate Data====<br />
<br />
*[https://docs.google.com/spreadsheets/d/1ZzbpDmkOI3IvGuKqyiQIP44sYJ89E3Zs9sLvjxvWMsc/edit#gid=sharing Particulates in Unaxis films @250C-2019]<br />
*[https://docs.google.com/spreadsheets/d/1fMebt-6BfAurcjMv1aDsmm6VgPqokU73_2ReZFqzEEk/edit#gid=sharing Particulates in Unaxis films @250C-2020]<br />
<br />
====Standard Recipes====<br />
<br />
*[https://docs.google.com/spreadsheets/d/1T_4gaJQ3wHSNptoAtFR1fN0ePwfw3PsQ0DLSjqGeyM4/edit#gid=sharing SiO2 LDR 250C Recipe-2020]<br />
*[https://docs.google.com/spreadsheets/d/1nsdGPpfyZfIesyYG1PIU9uYyuzQWrfpsvVWM6J_H6BI/edit#gid=sharing SiO2 HDR 250C Recipe-2020]<br />
*[https://docs.google.com/spreadsheets/d/1UTr93aWx0MjCwVBwRmYjPwo9ASluGQ-OrJhVG_R57aY/edit#gid=sharing SiN 250C Recipe-2020]<br />
*[https://docs.google.com/spreadsheets/d/1MXW7UNpTyk93ucOVQaSun5IX7QaUbSABNHNznb09qw8/edit#gid=sharing SiN LS 250C Recipe-2020]<br />
<br />
==SiO2 LDR 250C Deposition (Unaxis VLR)==<br />
''Low-Deposition Rate SiO<sub>2</sub>''<br />
====Historical Data====<br />
=====Thin-Film Properties=====<br />
This data is for 780sec long SiO2 LDR (low deposition rate) deposition, and cleaning time is 900sec, following the procedure [[here]].<br />
<br />
*[https://docs.google.com/spreadsheets/d/1wocoCPOOEDQcZbXJJNaZs1sr9dXBZpn1wUyglL8IQrI/edit#gid=sharing SiO2 LDR 250C 300nm Data-2019]<br />
*[https://docs.google.com/spreadsheets/d/1bU2Gu3x3DNyrq8skMAQZJCsra-IcoDCT0U5D135YPgc/edit#gid=sharing SiO2 LDR 250C 300nm Data-2020]<br />
<br />
=====Uniformity Data=====<br />
<br />
*[https://docs.google.com/spreadsheets/d/1Xi21OrargcNRthZ2fM_56APB8O599ctDfq5E_6B5Ft0/edit#gid=sharing Thickness Uniformity SiO2 LDR 250C 300nm-2019]<br />
*[https://docs.google.com/spreadsheets/d/1-ytu5R75FAXNfhJZTRuK2eRZyu_L6Hy1BWV2zN6_tRA/edit#gid=sharing Thickness Uniformity SiO2 LDR 250C 300nm-2020]<br />
<br />
==SiO2 HDR 250C Deposition (Unaxis VLR)==<br />
''High-Deposition Rate SiO<sub>2</sub>''<br />
====Historical Data====<br />
=====Thin-Film Properties=====<br />
This data is for 180sec long SiO2 HDR ( high deposition rate) deposition, and cleaning time is 900sec, following the procedure [[here]].<br />
<br />
*[https://docs.google.com/spreadsheets/d/16s-tUna9xrkKneK1lE-qSPuUHWlDmP6Qu3IngBXP3R8/edit#gid=sharing SiO2 HDR 250C 300nm Data-2019]<br />
*[https://docs.google.com/spreadsheets/d/1OxHi5r9ifNvF8ODpIk6aoRevb4RdbbykwPVMm1g-yi4/edit#gid=sharing SiO2 HDR 250C 300nm Data-2020]<br />
<br />
=====Uniformity Data=====<br />
<br />
*[https://docs.google.com/spreadsheets/d/1Mm_rsTm9xDQ50kZx6X6EZ5dTegUvinq0zFxRtE8B2R4/edit#gid=sharing Thickness Uniformity SiO2 HDR 250C 300nm-2019]<br />
*[https://docs.google.com/spreadsheets/d/1nzVeCKsmgL17zft6axQlixpvsEowJOG7qCnLQm_0XxE/edit#gid=sharing Thickness Uniformity SiO2 HDR 250C 300nm-2020]<br />
<br />
==SiN 250C deposition (Unaxis VLR)==<br />
====Historical Data====<br />
=====Thin-Film Properties=====<br />
This data is for 480sec long SiN deposition, and cleaning time is 1500sec, following the procedure [[here]].<br />
<br />
*[https://docs.google.com/spreadsheets/d/1VrgS0cB2OcdZVTCnDAesgQCLRaAgEB_Iajc_OrhXOo0/edit#gid=sharing SiN 250C 300nm Data-2020]<br />
<br />
=====Uniformity Data=====<br />
<br />
*[https://docs.google.com/spreadsheets/d/1YAx_Ix84xId8CAhDwZeFT7jLFUwg-BET9aBwg3DxUmQ/edit#gid=sharing Thickness Uniformity SiN 250C 300nm-2020]<br />
<br />
==SiN LS 250C Deposition (Unaxis VLR)==<br />
''Low Stress Silicon-Nitride''<br />
====Historical Data====<br />
''To Be Added''<br />
=====Thin-Film Properties=====<br />
This data is for 180sec long SiN LS (low stress) deposition, and cleaning time is 1500sec, following the procedure [[here]].<br />
<br />
*[https://docs.google.com/spreadsheets/d/1i2mE2K12EEulnCbO9KuU9PCcvHAmcGxTIXUF8x4IOWk/edit#gid=sharing SiN LS 250C 300nm Data-2020]<br />
<br />
=====Uniformity Data=====<br />
<br />
*[https://docs.google.com/spreadsheets/d/1NDyxH1i9COM2XTryLqYPE9yOekgRslAJUO7o56iTOEQ/edit#gid=sharing Thickness Uniformity SiN LS 250C 300nm-2020]<br />
<br />
==Cleaning Recipes (Unaxis VLR Dep)==<br />
You must edit the Post-Dep Clean recipe to correspond to your deposited thickness and material. See the [[ICP-PECVD (Unaxis VLR)#Documentation|Operating Procedure on the Unaxis Tool Page]] for details.<br />
<br />
*SiNx etches at 20nm/min<br />
*SiO2 etches at 40nm/min</div>
John d