PECVD 2 (Advanced Vacuum)

SiN deposition (PECVD #2)

  • Deposition Rate: ≈ 8.29 nm/min
  • Refractive Index: ≈ 1.955
  • Stress ≈ 498MPa
  • HF etch rate:~48nm/min

SiO2 deposition (PECVD #2)

  • Deposition Rate: ≈ 28.36 nm/min
  • Refractive Index: ≈ 1.473
  • Stress ≈ -256MPa
  • HF etch rate~582nm/min

LS SiN deposition (PECVD #2)

  • Deposition Rate: ≈ 8.17 nm/min
  • Refractive Index: ≈ 1.935
  • Stress ≈ -0.04MPa
  • HF etch rate~47nm/min

Amorphous-Si deposition (PECVD #2)