https://wiki.nanofab.ucsb.edu/w/index.php?title=OLD_-_PECVD2_Recipes&feed=atom&action=history
OLD - PECVD2 Recipes - Revision history
2024-03-28T18:58:04Z
Revision history for this page on the wiki
MediaWiki 1.35.13
https://wiki.nanofab.ucsb.edu/w/index.php?title=OLD_-_PECVD2_Recipes&diff=159694&oldid=prev
John d: John d moved page PECVD2 Recipes to OLD - PECVD2 Recipes without leaving a redirect: this page is not linked anywhere, looks like 2014 data only
2022-03-03T19:28:52Z
<p>John d moved page <a href="/w/index.php?title=PECVD2_Recipes&action=edit&redlink=1" class="new" title="PECVD2 Recipes (page does not exist)">PECVD2 Recipes</a> to <a href="/wiki/OLD_-_PECVD2_Recipes" title="OLD - PECVD2 Recipes">OLD - PECVD2 Recipes</a> without leaving a redirect: this page is not linked anywhere, looks like 2014 data only</p>
<table class="diff diff-contentalign-left diff-editfont-monospace" data-mw="interface">
<tr class="diff-title" lang="en">
<td colspan="1" style="background-color: #fff; color: #202122; text-align: center;">← Older revision</td>
<td colspan="1" style="background-color: #fff; color: #202122; text-align: center;">Revision as of 19:28, 3 March 2022</td>
</tr><tr><td colspan="2" class="diff-notice" lang="en"><div class="mw-diff-empty">(No difference)</div>
</td></tr></table>
John d
https://wiki.nanofab.ucsb.edu/w/index.php?title=OLD_-_PECVD2_Recipes&diff=153545&oldid=prev
Biljana: /* PECVD 2 (Advanced Vacuum) */
2015-01-09T18:44:36Z
<p><span dir="auto"><span class="autocomment">PECVD 2 (Advanced Vacuum)</span></span></p>
<table class="diff diff-contentalign-left diff-editfont-monospace" data-mw="interface">
<col class="diff-marker" />
<col class="diff-content" />
<col class="diff-marker" />
<col class="diff-content" />
<tr class="diff-title" lang="en">
<td colspan="2" style="background-color: #fff; color: #202122; text-align: center;">← Older revision</td>
<td colspan="2" style="background-color: #fff; color: #202122; text-align: center;">Revision as of 18:44, 9 January 2015</td>
</tr><tr>
<td colspan="2" class="diff-lineno">Line 4:</td>
<td colspan="2" class="diff-lineno">Line 4:</td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>*[[media: Photos Sheet1.pdf|Dirty platen]]</div></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>*[[media: Photos Sheet1.pdf|Dirty platen]]</div></td>
</tr>
<tr>
<td class="diff-marker">−</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #ffe49c; vertical-align: top; white-space: pre-wrap;"></td>
<td colspan="2" class="diff-empty"> </td>
</tr>
<tr>
<td class="diff-marker"><a class="mw-diff-movedpara-left" title="Paragraph was moved. Click to jump to new location." href="#movedpara_3_1_rhs">⚫</a></td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #ffe49c; vertical-align: top; white-space: pre-wrap;"><div><a name="movedpara_1_1_lhs"></a>== SiN deposition (PECVD #2) ==</div></td>
<td colspan="2" class="diff-empty"> </td>
</tr>
<tr>
<td class="diff-marker"><a class="mw-diff-movedpara-left" title="Paragraph was moved. Click to jump to new location." href="#movedpara_3_2_rhs">⚫</a></td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #ffe49c; vertical-align: top; white-space: pre-wrap;"><div><a name="movedpara_1_2_lhs"></a>*[[media:NewAdvPECVD-Nitride2 300C standard recipe.pdf|Nitride2 Standard Recipe]]</div></td>
<td colspan="2" class="diff-empty"> </td>
</tr>
<tr>
<td class="diff-marker"><a class="mw-diff-movedpara-left" title="Paragraph was moved. Click to jump to new location." href="#movedpara_3_3_rhs">⚫</a></td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #ffe49c; vertical-align: top; white-space: pre-wrap;"><div><a name="movedpara_1_3_lhs"></a>*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dDE0R3FlenNPa2txNmRldTczMXZNNnc#gid=sharing Nitride2 Data 2014]</div></td>
<td colspan="2" class="diff-empty"> </td>
</tr>
<tr>
<td class="diff-marker"><a class="mw-diff-movedpara-left" title="Paragraph was moved. Click to jump to new location." href="#movedpara_3_4_rhs">⚫</a></td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #ffe49c; vertical-align: top; white-space: pre-wrap;"><div><a name="movedpara_1_4_lhs"></a>*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dERkYm85bGtYQVpjVk5GTGJuMkg2anc&usp=drive_web#gid=sharing Nitride2 Thickness uniformity 2014]</div></td>
<td colspan="2" class="diff-empty"> </td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>== SiO<sub>2</sub> deposition (PECVD #2) ==</div></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>== SiO<sub>2</sub> deposition (PECVD #2) ==</div></td>
</tr>
<tr>
<td colspan="2" class="diff-lineno">Line 14:</td>
<td colspan="2" class="diff-lineno">Line 9:</td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dGJZaGtDTVRqa1BRdW5iU1N1Y01jd0E&usp=drive_web#gid=sharing Oxide Data 2014]</div></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dGJZaGtDTVRqa1BRdW5iU1N1Y01jd0E&usp=drive_web#gid=sharing Oxide Data 2014]</div></td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dDRjSHEtYUZRUTg4azE2U0JGUTg2M1E#gid=sharing Oxide Thickness uniformity 2014]</div></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dDRjSHEtYUZRUTg4azE2U0JGUTg2M1E#gid=sharing Oxide Thickness uniformity 2014]</div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker"><a class="mw-diff-movedpara-right" title="Paragraph was moved. Click to jump to old location." href="#movedpara_1_1_lhs">⚫</a></td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div><a name="movedpara_3_1_rhs"></a>== SiN deposition (PECVD #2) ==</div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker"><a class="mw-diff-movedpara-right" title="Paragraph was moved. Click to jump to old location." href="#movedpara_1_2_lhs">⚫</a></td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div><a name="movedpara_3_2_rhs"></a>*[[media:NewAdvPECVD-Nitride2 300C standard recipe.pdf|Nitride2 Standard Recipe]]</div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker"><a class="mw-diff-movedpara-right" title="Paragraph was moved. Click to jump to old location." href="#movedpara_1_3_lhs">⚫</a></td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div><a name="movedpara_3_3_rhs"></a>*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dDE0R3FlenNPa2txNmRldTczMXZNNnc#gid=sharing Nitride2 Data 2014]</div></td>
</tr>
<tr>
<td colspan="2" class="diff-empty"> </td>
<td class="diff-marker"><a class="mw-diff-movedpara-right" title="Paragraph was moved. Click to jump to old location." href="#movedpara_1_4_lhs">⚫</a></td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div><a name="movedpara_3_4_rhs"></a>*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dERkYm85bGtYQVpjVk5GTGJuMkg2anc&usp=drive_web#gid=sharing Nitride2 Thickness uniformity 2014]</div></td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>==LS SiN deposition (PECVD #2) ==</div></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>==LS SiN deposition (PECVD #2) ==</div></td>
</tr>
</table>
Biljana
https://wiki.nanofab.ucsb.edu/w/index.php?title=OLD_-_PECVD2_Recipes&diff=153487&oldid=prev
Biljana: /* LS SiN deposition (PECVD #2) */
2014-12-11T21:40:56Z
<p><span dir="auto"><span class="autocomment">LS SiN deposition (PECVD #2)</span></span></p>
<table class="diff diff-contentalign-left diff-editfont-monospace" data-mw="interface">
<col class="diff-marker" />
<col class="diff-content" />
<col class="diff-marker" />
<col class="diff-content" />
<tr class="diff-title" lang="en">
<td colspan="2" style="background-color: #fff; color: #202122; text-align: center;">← Older revision</td>
<td colspan="2" style="background-color: #fff; color: #202122; text-align: center;">Revision as of 21:40, 11 December 2014</td>
</tr><tr>
<td colspan="2" class="diff-lineno">Line 16:</td>
<td colspan="2" class="diff-lineno">Line 16:</td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>==LS SiN deposition (PECVD #2) ==</div></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>==LS SiN deposition (PECVD #2) ==</div></td>
</tr>
<tr>
<td class="diff-marker">−</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #ffe49c; vertical-align: top; white-space: pre-wrap;"><div>*[[media:<del class="diffchange diffchange-inline">AdvPECVD</del>-LS Nitride2 300C standard recipe.pdf|LS Nitride2 Standard Recipe]]</div></td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>*[[media:<ins class="diffchange diffchange-inline">NewAdvPECVD</ins>-LS Nitride2 300C standard recipe.pdf|LS Nitride2 Standard Recipe]]</div></td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dEZvWVhzS1pHUXZkOGcyQWZ4LTNBWGc&usp=drive_web#gid=sharing LS Nitride2 Data 2014]</div></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dEZvWVhzS1pHUXZkOGcyQWZ4LTNBWGc&usp=drive_web#gid=sharing LS Nitride2 Data 2014]</div></td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dENSak1ZNnVaVTFEQTBzdDJMSDlDTFE&usp=drive_web#gid=1=sharing LS Nitride2 Thickness uniformity 2014]</div></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dENSak1ZNnVaVTFEQTBzdDJMSDlDTFE&usp=drive_web#gid=1=sharing LS Nitride2 Thickness uniformity 2014]</div></td>
</tr>
</table>
Biljana
https://wiki.nanofab.ucsb.edu/w/index.php?title=OLD_-_PECVD2_Recipes&diff=153486&oldid=prev
Biljana: /* LS SiN deposition (PECVD #2) */
2014-12-11T19:46:46Z
<p><span dir="auto"><span class="autocomment">LS SiN deposition (PECVD #2)</span></span></p>
<table class="diff diff-contentalign-left diff-editfont-monospace" data-mw="interface">
<col class="diff-marker" />
<col class="diff-content" />
<col class="diff-marker" />
<col class="diff-content" />
<tr class="diff-title" lang="en">
<td colspan="2" style="background-color: #fff; color: #202122; text-align: center;">← Older revision</td>
<td colspan="2" style="background-color: #fff; color: #202122; text-align: center;">Revision as of 19:46, 11 December 2014</td>
</tr><tr>
<td colspan="2" class="diff-lineno">Line 16:</td>
<td colspan="2" class="diff-lineno">Line 16:</td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>==LS SiN deposition (PECVD #2) ==</div></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>==LS SiN deposition (PECVD #2) ==</div></td>
</tr>
<tr>
<td class="diff-marker">−</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #ffe49c; vertical-align: top; white-space: pre-wrap;"></td>
<td colspan="2" class="diff-empty"> </td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>*[[media:AdvPECVD-LS Nitride2 300C standard recipe.pdf|LS Nitride2 Standard Recipe]]</div></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>*[[media:AdvPECVD-LS Nitride2 300C standard recipe.pdf|LS Nitride2 Standard Recipe]]</div></td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dEZvWVhzS1pHUXZkOGcyQWZ4LTNBWGc&usp=drive_web#gid=sharing LS Nitride2 Data 2014]</div></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dEZvWVhzS1pHUXZkOGcyQWZ4LTNBWGc&usp=drive_web#gid=sharing LS Nitride2 Data 2014]</div></td>
</tr>
</table>
Biljana
https://wiki.nanofab.ucsb.edu/w/index.php?title=OLD_-_PECVD2_Recipes&diff=153485&oldid=prev
Biljana: /* LS SiN deposition (PECVD #2) */
2014-12-11T19:46:37Z
<p><span dir="auto"><span class="autocomment">LS SiN deposition (PECVD #2)</span></span></p>
<table class="diff diff-contentalign-left diff-editfont-monospace" data-mw="interface">
<col class="diff-marker" />
<col class="diff-content" />
<col class="diff-marker" />
<col class="diff-content" />
<tr class="diff-title" lang="en">
<td colspan="2" style="background-color: #fff; color: #202122; text-align: center;">← Older revision</td>
<td colspan="2" style="background-color: #fff; color: #202122; text-align: center;">Revision as of 19:46, 11 December 2014</td>
</tr><tr>
<td colspan="2" class="diff-lineno">Line 18:</td>
<td colspan="2" class="diff-lineno">Line 18:</td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>*[[media:AdvPECVD-LS Nitride2 300C standard recipe.pdf|LS Nitride2 Standard Recipe]]</div></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>*[[media:AdvPECVD-LS Nitride2 300C standard recipe.pdf|LS Nitride2 Standard Recipe]]</div></td>
</tr>
<tr>
<td class="diff-marker">−</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #ffe49c; vertical-align: top; white-space: pre-wrap;"><div>*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dEZvWVhzS1pHUXZkOGcyQWZ4LTNBWGc&usp=drive_web#gid=sharing LS Nitride2 Data<del class="diffchange diffchange-inline"> December</del> 2014]</div></td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dEZvWVhzS1pHUXZkOGcyQWZ4LTNBWGc&usp=drive_web#gid=sharing LS Nitride2 Data 2014]</div></td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dENSak1ZNnVaVTFEQTBzdDJMSDlDTFE&usp=drive_web#gid=1=sharing LS Nitride2 Thickness uniformity 2014]</div></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dENSak1ZNnVaVTFEQTBzdDJMSDlDTFE&usp=drive_web#gid=1=sharing LS Nitride2 Thickness uniformity 2014]</div></td>
</tr>
<tr>
<td class="diff-marker">−</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #ffe49c; vertical-align: top; white-space: pre-wrap;"></td>
<td colspan="2" class="diff-empty"> </td>
</tr>
<tr>
<td class="diff-marker">−</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #ffe49c; vertical-align: top; white-space: pre-wrap;"><div>*Deposition Rate: ≈ 7.87 nm/min (users must calibrate this prior to critical deps)</div></td>
<td colspan="2" class="diff-empty"> </td>
</tr>
<tr>
<td class="diff-marker">−</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #ffe49c; vertical-align: top; white-space: pre-wrap;"><div>*Refractive Index: ≈ 1.938</div></td>
<td colspan="2" class="diff-empty"> </td>
</tr>
<tr>
<td class="diff-marker">−</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #ffe49c; vertical-align: top; white-space: pre-wrap;"><div>*Stress ≈ 1.76MPa</div></td>
<td colspan="2" class="diff-empty"> </td>
</tr>
<tr>
<td class="diff-marker">−</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #ffe49c; vertical-align: top; white-space: pre-wrap;"><div>*HF etch rate~47nm/min</div></td>
<td colspan="2" class="diff-empty"> </td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>== Amorphous-Si deposition (PECVD #2) ==</div></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>== Amorphous-Si deposition (PECVD #2) ==</div></td>
</tr>
</table>
Biljana
https://wiki.nanofab.ucsb.edu/w/index.php?title=OLD_-_PECVD2_Recipes&diff=153484&oldid=prev
Biljana: /* Photos */
2014-12-11T19:11:21Z
<p><span dir="auto"><span class="autocomment">Photos</span></span></p>
<table class="diff diff-contentalign-left diff-editfont-monospace" data-mw="interface">
<col class="diff-marker" />
<col class="diff-content" />
<col class="diff-marker" />
<col class="diff-content" />
<tr class="diff-title" lang="en">
<td colspan="2" style="background-color: #fff; color: #202122; text-align: center;">← Older revision</td>
<td colspan="2" style="background-color: #fff; color: #202122; text-align: center;">Revision as of 19:11, 11 December 2014</td>
</tr><tr>
<td colspan="2" class="diff-lineno">Line 3:</td>
<td colspan="2" class="diff-lineno">Line 3:</td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>==Photos==</div></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>==Photos==</div></td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
</tr>
<tr>
<td class="diff-marker">−</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #ffe49c; vertical-align: top; white-space: pre-wrap;"><div>*[[media: <del class="diffchange diffchange-inline">Dirty</del> <del class="diffchange diffchange-inline">platen photos</del>.pdf|Dirty platen]]</div></td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>*[[media: <ins class="diffchange diffchange-inline">Photos</ins> <ins class="diffchange diffchange-inline">Sheet1</ins>.pdf|Dirty platen]]</div></td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>== SiN deposition (PECVD #2) ==</div></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>== SiN deposition (PECVD #2) ==</div></td>
</tr>
</table>
Biljana
https://wiki.nanofab.ucsb.edu/w/index.php?title=OLD_-_PECVD2_Recipes&diff=153481&oldid=prev
Biljana: /* SiN deposition (PECVD #2) */
2014-12-11T19:01:32Z
<p><span dir="auto"><span class="autocomment">SiN deposition (PECVD #2)</span></span></p>
<table class="diff diff-contentalign-left diff-editfont-monospace" data-mw="interface">
<col class="diff-marker" />
<col class="diff-content" />
<col class="diff-marker" />
<col class="diff-content" />
<tr class="diff-title" lang="en">
<td colspan="2" style="background-color: #fff; color: #202122; text-align: center;">← Older revision</td>
<td colspan="2" style="background-color: #fff; color: #202122; text-align: center;">Revision as of 19:01, 11 December 2014</td>
</tr><tr>
<td colspan="2" class="diff-lineno">Line 6:</td>
<td colspan="2" class="diff-lineno">Line 6:</td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>== SiN deposition (PECVD #2) ==</div></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>== SiN deposition (PECVD #2) ==</div></td>
</tr>
<tr>
<td class="diff-marker">−</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #ffe49c; vertical-align: top; white-space: pre-wrap;"><div>*[[media:<del class="diffchange diffchange-inline">New Advanced PECVD</del>-Nitride2 300C standard recipe.pdf|Nitride2 Standard Recipe]]</div></td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>*[[media:<ins class="diffchange diffchange-inline">NewAdvPECVD</ins>-Nitride2 300C standard recipe.pdf|Nitride2 Standard Recipe]]</div></td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dDE0R3FlenNPa2txNmRldTczMXZNNnc#gid=sharing Nitride2 Data 2014]</div></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dDE0R3FlenNPa2txNmRldTczMXZNNnc#gid=sharing Nitride2 Data 2014]</div></td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dERkYm85bGtYQVpjVk5GTGJuMkg2anc&usp=drive_web#gid=sharing Nitride2 Thickness uniformity 2014]</div></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dERkYm85bGtYQVpjVk5GTGJuMkg2anc&usp=drive_web#gid=sharing Nitride2 Thickness uniformity 2014]</div></td>
</tr>
</table>
Biljana
https://wiki.nanofab.ucsb.edu/w/index.php?title=OLD_-_PECVD2_Recipes&diff=153480&oldid=prev
Biljana: /* SiN deposition (PECVD #2) */
2014-12-11T17:54:31Z
<p><span dir="auto"><span class="autocomment">SiN deposition (PECVD #2)</span></span></p>
<table class="diff diff-contentalign-left diff-editfont-monospace" data-mw="interface">
<col class="diff-marker" />
<col class="diff-content" />
<col class="diff-marker" />
<col class="diff-content" />
<tr class="diff-title" lang="en">
<td colspan="2" style="background-color: #fff; color: #202122; text-align: center;">← Older revision</td>
<td colspan="2" style="background-color: #fff; color: #202122; text-align: center;">Revision as of 17:54, 11 December 2014</td>
</tr><tr>
<td colspan="2" class="diff-lineno">Line 7:</td>
<td colspan="2" class="diff-lineno">Line 7:</td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>== SiN deposition (PECVD #2) ==</div></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>== SiN deposition (PECVD #2) ==</div></td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>*[[media:New Advanced PECVD-Nitride2 300C standard recipe.pdf|Nitride2 Standard Recipe]]</div></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>*[[media:New Advanced PECVD-Nitride2 300C standard recipe.pdf|Nitride2 Standard Recipe]]</div></td>
</tr>
<tr>
<td class="diff-marker">−</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #ffe49c; vertical-align: top; white-space: pre-wrap;"><div>*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dDE0R3FlenNPa2txNmRldTczMXZNNnc#gid=sharing Nitride2 Data<del class="diffchange diffchange-inline"> Devcember</del> 2014]</div></td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dDE0R3FlenNPa2txNmRldTczMXZNNnc#gid=sharing Nitride2 Data 2014]</div></td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dERkYm85bGtYQVpjVk5GTGJuMkg2anc&usp=drive_web#gid=sharing Nitride2 Thickness uniformity 2014]</div></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dERkYm85bGtYQVpjVk5GTGJuMkg2anc&usp=drive_web#gid=sharing Nitride2 Thickness uniformity 2014]</div></td>
</tr>
<tr>
<td class="diff-marker">−</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #ffe49c; vertical-align: top; white-space: pre-wrap;"></td>
<td colspan="2" class="diff-empty"> </td>
</tr>
<tr>
<td class="diff-marker">−</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #ffe49c; vertical-align: top; white-space: pre-wrap;"><div>*Deposition Rate: ≈ 7.93 nm/min (users must calibrate this prior to critical deps)</div></td>
<td colspan="2" class="diff-empty"> </td>
</tr>
<tr>
<td class="diff-marker">−</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #ffe49c; vertical-align: top; white-space: pre-wrap;"><div>*Refractive Index: ≈ 1.961</div></td>
<td colspan="2" class="diff-empty"> </td>
</tr>
<tr>
<td class="diff-marker">−</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #ffe49c; vertical-align: top; white-space: pre-wrap;"><div>*Stress ≈ 495MPa</div></td>
<td colspan="2" class="diff-empty"> </td>
</tr>
<tr>
<td class="diff-marker">−</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #ffe49c; vertical-align: top; white-space: pre-wrap;"><div>*HF etch rate:~49nm/min</div></td>
<td colspan="2" class="diff-empty"> </td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>== SiO<sub>2</sub> deposition (PECVD #2) ==</div></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>== SiO<sub>2</sub> deposition (PECVD #2) ==</div></td>
</tr>
</table>
Biljana
https://wiki.nanofab.ucsb.edu/w/index.php?title=OLD_-_PECVD2_Recipes&diff=153478&oldid=prev
Biljana: /* SiO2 deposition (PECVD #2) */
2014-12-11T17:52:33Z
<p><span dir="auto"><span class="autocomment">SiO2 deposition (PECVD #2)</span></span></p>
<table class="diff diff-contentalign-left diff-editfont-monospace" data-mw="interface">
<col class="diff-marker" />
<col class="diff-content" />
<col class="diff-marker" />
<col class="diff-content" />
<tr class="diff-title" lang="en">
<td colspan="2" style="background-color: #fff; color: #202122; text-align: center;">← Older revision</td>
<td colspan="2" style="background-color: #fff; color: #202122; text-align: center;">Revision as of 17:52, 11 December 2014</td>
</tr><tr>
<td colspan="2" class="diff-lineno">Line 16:</td>
<td colspan="2" class="diff-lineno">Line 16:</td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>== SiO<sub>2</sub> deposition (PECVD #2) ==</div></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>== SiO<sub>2</sub> deposition (PECVD #2) ==</div></td>
</tr>
<tr>
<td class="diff-marker">−</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #ffe49c; vertical-align: top; white-space: pre-wrap;"><div>*[[media:<del class="diffchange diffchange-inline">Advanced PECVD</del> OXIDE 300C standard recipe<del class="diffchange diffchange-inline"> OXIDE Standard Recipe</del>.pdf|Oxide Standard Recipe]]</div></td>
<td class="diff-marker">+</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;"><div>*[[media:<ins class="diffchange diffchange-inline">NewAdvPECVD</ins> OXIDE 300C standard recipe.pdf|Oxide Standard Recipe]]</div></td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dGJZaGtDTVRqa1BRdW5iU1N1Y01jd0E&usp=drive_web#gid=sharing Oxide Data 2014]</div></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dGJZaGtDTVRqa1BRdW5iU1N1Y01jd0E&usp=drive_web#gid=sharing Oxide Data 2014]</div></td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dDRjSHEtYUZRUTg4azE2U0JGUTg2M1E#gid=sharing Oxide Thickness uniformity 2014]</div></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dDRjSHEtYUZRUTg4azE2U0JGUTg2M1E#gid=sharing Oxide Thickness uniformity 2014]</div></td>
</tr>
</table>
Biljana
https://wiki.nanofab.ucsb.edu/w/index.php?title=OLD_-_PECVD2_Recipes&diff=153477&oldid=prev
Biljana: /* SiO2 deposition (PECVD #2) */
2014-12-11T17:12:57Z
<p><span dir="auto"><span class="autocomment">SiO2 deposition (PECVD #2)</span></span></p>
<table class="diff diff-contentalign-left diff-editfont-monospace" data-mw="interface">
<col class="diff-marker" />
<col class="diff-content" />
<col class="diff-marker" />
<col class="diff-content" />
<tr class="diff-title" lang="en">
<td colspan="2" style="background-color: #fff; color: #202122; text-align: center;">← Older revision</td>
<td colspan="2" style="background-color: #fff; color: #202122; text-align: center;">Revision as of 17:12, 11 December 2014</td>
</tr><tr>
<td colspan="2" class="diff-lineno">Line 19:</td>
<td colspan="2" class="diff-lineno">Line 19:</td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dGJZaGtDTVRqa1BRdW5iU1N1Y01jd0E&usp=drive_web#gid=sharing Oxide Data 2014]</div></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dGJZaGtDTVRqa1BRdW5iU1N1Y01jd0E&usp=drive_web#gid=sharing Oxide Data 2014]</div></td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dDRjSHEtYUZRUTg4azE2U0JGUTg2M1E#gid=sharing Oxide Thickness uniformity 2014]</div></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dDRjSHEtYUZRUTg4azE2U0JGUTg2M1E#gid=sharing Oxide Thickness uniformity 2014]</div></td>
</tr>
<tr>
<td class="diff-marker">−</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #ffe49c; vertical-align: top; white-space: pre-wrap;"></td>
<td colspan="2" class="diff-empty"> </td>
</tr>
<tr>
<td class="diff-marker">−</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #ffe49c; vertical-align: top; white-space: pre-wrap;"><div>*Deposition Rate: ≈ 28.64 nm/min (users must calibrate this prior to critical deps)</div></td>
<td colspan="2" class="diff-empty"> </td>
</tr>
<tr>
<td class="diff-marker">−</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #ffe49c; vertical-align: top; white-space: pre-wrap;"><div>*Refractive Index: ≈ 1.475</div></td>
<td colspan="2" class="diff-empty"> </td>
</tr>
<tr>
<td class="diff-marker">−</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #ffe49c; vertical-align: top; white-space: pre-wrap;"><div>*Stress ≈ -260MPa</div></td>
<td colspan="2" class="diff-empty"> </td>
</tr>
<tr>
<td class="diff-marker">−</td>
<td style="color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #ffe49c; vertical-align: top; white-space: pre-wrap;"><div>*HF etch rate~623nm/min</div></td>
<td colspan="2" class="diff-empty"> </td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"></td>
</tr>
<tr>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>==LS SiN deposition (PECVD #2) ==</div></td>
<td class="diff-marker"> </td>
<td style="background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;"><div>==LS SiN deposition (PECVD #2) ==</div></td>
</tr>
</table>
Biljana