Difference between revisions of "OLD - PECVD2 Recipes"
Jump to navigation
Jump to search
Line 23: | Line 23: | ||
*[[media:AdvPECVD-LS Nitride2 300C standard recipe.pdf|LS Nitride2 Standard Recipe]] |
*[[media:AdvPECVD-LS Nitride2 300C standard recipe.pdf|LS Nitride2 Standard Recipe]] |
||
− | *[[media:New Advanced PECVD LS NITRIDE2 April 2014.pdf|LS Nitride2 Data (Deposition Rate, Refractive Index, Stress, HF etch rate )]] |
||
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dEZvWVhzS1pHUXZkOGcyQWZ4LTNBWGc&usp=drive_web#gid=sharing LS Nitride2 Data April 2014] |
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dEZvWVhzS1pHUXZkOGcyQWZ4LTNBWGc&usp=drive_web#gid=sharing LS Nitride2 Data April 2014] |
||
Revision as of 18:44, 21 May 2014
PECVD 2 (Advanced Vacuum)
SiN deposition (PECVD #2)
- Deposition Rate: ≈ 8.29 nm/min
- Refractive Index: ≈ 1.955
- Stress ≈ 498MPa
- HF etch rate:~48nm/min
SiO2 deposition (PECVD #2)
- Deposition Rate: ≈ 28.36 nm/min
- Refractive Index: ≈ 1.473
- Stress ≈ -256MPa
- HF etch rate~582nm/min
LS SiN deposition (PECVD #2)
- Deposition Rate: ≈ 8.17 nm/min
- Refractive Index: ≈ 1.935
- Stress ≈ -0.04MPa
- HF etch rate~47nm/min